Fluoride Inside: Syntheses, Structure, and Optical Properties of the REFWO4 Representatives with RE = Y, Sm–Lu Authors: Benjamin Knies, Priya Pandey, Markus Suta, Ingo Hartenbach Published: 2026 ABSTRACT The reactions of WO3, RE 2O3, and REF3 (RE = Y, Sm–Lu) with an excess of CsBr as flux lead to the formations of coarse single crystals with the composition REFWO4. In the crystal structure (space group P1̅; a = 471–467, b = 617–589, c = 694–676 pm; α ≈ 89°, β = 83–81°, γ ≈ 75°; Z = 2), 8-fold coordinated RE 3+ cations are present in the shape of distorted trigonal dodecahedra consisting of five O2– and three F– anions. One of the latter contacts is gradually detached throughout the series from RE = Sm to Lu, so that the coordination number of Sm3+ in SmFWO4 can be considered as eight, while for LuFWO4 the coordination number of Lu3+ is more accurately described as seven plus one. The W6+ cations are surrounded by six O2– anions in distorted octahedral shapes, and these polyhedra are fused together via common edges chains running along [100]. Both YFWO4 and GdFWO4 were activated with Eu3+ and Tb3+ cations to investigate the usability of these compounds as host materials for luminescence. Besides steady-state excitation and emission spectra, time-resolved measurements at 80 K and at room temperature were performed. Introduction The structural chemistry of rare-earth metal tungstates is very diverse and also rather thoroughly investigated. These compounds represent interesting host materials for luminescence applications, such as upconversion processes or in lighting. Halide derivatives of rare-earth metal tungstates, on the other hand, have not experienced such wide-range research interests despite the first representative of this class of compounds, Pr3Cl3[WO6], being known since 1969. In the early 1980s, the group around Brixner performed thorough investigations of several lanthanum and gadolinium chloride tungstates, − and after that another 30-year hiatus of this research topic occurred. While the chloride derivatives with the formula RECl­[WO4] of the larger lanthanoids experience some crystallographic difficulties with respect to the description in the correct unit cell and crystal system, the representatives of the smaller metals RE = Gd–Er crystallize isotypically in the monoclinic system, while those of the smallest RE = Tm–Lu also crystallize isotypically in the triclinic system. Furthermore, bromide derivatives were investigated for the first time with the REBr­[WO4] series for the smaller elements RE = Y, Gd–Lu again being isotypic to each other in a so far unique triclinic structure. Some research was also dedicated to the representatives of the larger metals, which unfortunately experience the same crystallographic difficulties as the chloride congeners. , All the previously mentioned compounds contain non-condensed tetrahedral [WO4]2– entities; however, the capacity of hexavalent tungsten to enlarge its coordination number from four to five or six is realized in the RE 3Cl3[WO6] series, ,,,,, in which non-condensed trigonal prismatic [WO6]6– units are present. While the extension toward iodine derivatives has so far not been successful due to iodide being a strong enough reduction agent to reduce the hexavalent tungsten during the synthesis process, the extension toward the fluoride representatives mostly suffered from side reactions of the F– anions with container materials in solid-state reactions or from poor crystallinity of the obtained products in solvochemical reactions. A first success in synthesizing a fluoride derivative of a rare-earth metal tungstate was achieved by high-pressure synthesis, yielding few single crystals of Gd5FW3O16. After many more failed attempts of solid-state, hydrothermal, or solvochemical syntheses, the utilization of cesium bromide as flux in high-temperature preparations, which has proven to be successful in synthesizing fluoride-containing rare-earth metal compounds with complex anions, such as REF­[SeO3] (RE = Y, Ho–Lu) in the past, resulted in the title compounds REFWO4 (RE = Y, Sm–Lu). Thus, the title compounds represent the first series of representatives in the quaternary system RE–W–F–O. Other than for the chloride and bromide derivatives, the rare-earth fluoride tungstates do not crystallize isotypically to their molybdate congeners REF­[MoO4] (RE = Y, Ce–Nd, Sm–Tm) but with a unique structure type and condensed tungstate octahedra instead of tetrahedral [WO4]2– units. Results and Discussion Crystal Structure The REFWO4 representatives with RE = Y, Sm–Lu crystallize in the triclinic space group P1̅ (no. 2) with two formula units per unit cell and the following ranges of lattice parameters: a = 471–467 pm, b = 617–589 pm, c = 694–676 pm, α ≈ 89°, β = 83–81°, γ ≈ 75°. The unit cell contains one crystallographically unique RE 3+ site with an 8-fold anionic environment consisting of five oxide and three fluoride anions in a shape best resembling a trigonal dodecahedron (see Figure , left) according to the program Polynator 1.7 (with deviations from the ideal one in the range of δ = 7.154–8.563 from RE = Sm to Lu). Distorted trigonal [REO5F3] dodecahedron (left) and distorted didigonal [WO6] scalenohedron in the crystal structures of the REFWO4 representatives with RE = Y, Sm–Lu (right). Ellipsoid representations at 95% with respect to the YFWO4 data. The interatomic distances within the [REO5F3] polyhedra are listed in Table . They follow the lanthanoid contraction, i.e., becoming smaller throughout the series with the exception of the RE···F″ distance, which increases from SmFWO4 to LuFWO4 (see Figure ) due to the diminished coordinative demand of the heavier rare-earth elements. This decrease in the effective coordination number (ECoN) was also calculated with the program CHARDI, , where the F″ ligand exhibits a contribution of 0.72 to the ECoN value of 7.83 for the Sm3+ cations in SmFWO4, while in LuFWO4 the same ligand merely contributes 0.11 to the ECoN value of 7.13 for the Lu3+ cations. 1Interatomic Distances (d/pm) within the [REO5F3] Polyhedra Throughout REFWO4 Series (RE = Y, Sm–Lu) RE RE–O4 RE–O1 RE–F RE–O2 RE–F′ RE–O2′ RE–O3 RE···F″Y225.4(2)227.1(3)229.3(2)230.4(2)231.6(2)237.4(2)239.0(2)264.1(2)Sm232.4(4)234.8(4)238.2(3)238.1(4)241.4(4)243.6(4)244.7(4)255.6(4)Eu230.7(3)233.0(3)236.3(2)236.1(3)240.4(3)242.0(3)243.5(3)255.9(3)Gd230.1(3)232.2(3)235.1(3)235.8(3)239.2(3)241.6(3)242.8(3)256.4(3)Tb228.2(3)230.0(3)233.0(3)233.4(3)237.0(3)239.6(3)240.9(3)258.5(3)Dy226.5(2)228.6(2)231.3(2)232.6(2)234.7(2)238.9(2)240.5(2)260.3(2)Ho225.7(3)227.8(3)230.4(3)231.7(3)233.1(3)238.2(3)239.8(3)262.4(3)Er224.7(2)226.3(2)228.7(2)229.2(1)230.5(2)236.8(2)238.0(2)265.5(2)Tm223.7(3)225.0(3)227.3(3)228.1(3)228.6(3)235.4(3)237.0(3)268.8(3)Yb222.4(3)224.0(3)225.0(2)227.1(3)226.9(3)234.7(3)235.5(3)271.5(3)Lu221.9(4)222.7(4)224.4(4)226.2(4)224.7(4)233.9(4)234.7(4)275.7(4) Interatomic Distances (d/pm) within the [REO5F3] Polyhedra Throughout REFWO4 Series (RE = Y, Sm–Lu) Trend of the interatomic distance between RE 3+ and the farthest fluoride ligand F″ (red) compared to the distance to the closest F (blue). The hexavalent tungsten cations are surrounded by six oxygen atoms in a distorted octahedral, or more accurately termed as distorted didigonal scalenohedral fashion (see Figure , right), according to the program Polynator 1.7 (the deviation from the ideal didigonal scalenohedron ranges about δ = 9.5 ± 0.3 throughout the whole series). The W6+–O2– bond lengths (see Table ) exhibit the typical behavior found for edge-connected octahedral tungstate entities, i.e., the terminal oxide anions O1 and O2 show the shortest bond lengths, while for the connecting edges O3–O3′ and O4–O4′, one shorter (between 180 and 190 pm) and one longer distance (between 210 and 225 pm) are found. The previously mentioned edge connection leads to {∞1[WO4/2eO2/1t]2−} strands along [100] (see Figure , top), which remain basically similar-sized throughout the whole series, i.e., they are not affected by the lanthanoid contraction. The partial structure of the RE 3+ cations and the F– anions can also be described as chains, built up by [RE 2F2] rhombi being linked via the longest RE–F″ distance to a ladder-like arrangement, running along the crystallographic a axis as well (see Figure , bottom). While the tungstate strand remains spatially rigid throughout the whole series, the shrinking ionic radius of the RE 3+ cations leads to the RE–F″ becoming gradually detached. As a consequence, the a lattice parameter does not change significantly from SmFWO4 to LuFWO4, while the other two steadily decrease (see Figure ). Both strands are arranged in primitive rod packings, interpenetrating each other to build up the three-dimensional structure (see Figure ). {∞1[WO4/2eO2/1t]2−} strands (top) and {∞1[FRE3/3]2+} chains (bottom) running along the a axis in the structures of the REFWO4 representatives with RE = Y, Sm–Lu. The longest RE 3+–F– distances in the latter are displayed in dashed bonds. 2Bond Lengths (d/pm) within Tungstate Entities throughout the REFWO4 Series (RE = Y, Sm–Lu) RE W–O1W–O2W–O3W–O4W–O4′W–O3′Y174.0(3)183.7(2)184.3(2)190.0(2)211.1(2)224.7(2)Sm174.1(4)183.2(4)183.8(4)189.9(4)210.5(4)225.9(4)Eu174.2(3)183.9(3)184.6(3)190.3(3)210.3(3)225.1(3)Gd173.6(3)182.6(3)184.0(3)189.8(3)210.7(3)225.9(3)Tb174.3(3)184.0(3)184.3(3)190.2(3)210.5(3)225.3(3)Dy173.7(2)182.8(2)184.2(2)190.4(2)210.3(2)225.1(2)Ho174.0(3)182.7(3)184.5(3)190.1(3)211.1(3)224.9(3)Er173.9(2)183.8(2)185.0(2)189.9(2)210.9(2)224.5(2)Tm173.4(3)183.9(3)184.6(3)189.9(3)211.3(3)224.4(3)Yb173.6(2)183.2(3)184.4(3)190.0(3)210.9(3)224.2(2)Lu174.0(4)183.6(4)184.6(4)190.2(4)211.3(4)224.2(4) Bond Lengths (d/pm) within Tungstate Entities throughout the REFWO4 Series (RE = Y, Sm–Lu) Representation of the unit cell dimensions versus the ionic radius of the respective rare-earth metal cation (for C.N. = 8) and linear regression of the values. While the b and the c axes steadily decrease from the Sm to the Lu congener, the a axis remains basically constant, exhibiting a minor upward trend. View at the crystal structure of the REFWO4 representatives with RE = Y, Sm–Lu along [100], emphasizing the interpenetrating rod packing of the {∞1[WO4/2eO2/1t]2−} strands and the {∞1[FRE3/3]2+} chains. Distinguishing fluoride from oxide anions by means of single-crystal X-ray diffraction is not always unambiguous due to their similar scattering powers. Due to electroneutrality reasons, the F:O ratio of 1:4 has to be maintained in the compounds; however, the question of the correct allocation of the elements to their reported position remains. Two of the oxygen atoms surrounding the W6+ cations serve in an interconnecting capacity; thus, due to chemical reasons, it is highly unlikely that these oxide anions would be even partially substituted by fluoride. Attempts to refine the crystal structures with a partial or complete fluoride/oxide exchange on the remaining positions F, O1, and O2, respectively, result in significantly higher residual values as well as in too low (for refining oxygen on the fluoride position) or rather high anisotropic displacement parameters (for refining fluorine on the O1 or the O2 position), respectively. This was also observed during the refinement of the respective rare-earth-metal-fluoride molybdates REF­[MoO4] − and REFMo2O7. , Furthermore, bond-valence calculations with the program CHARDI result in a 300 to 600% higher deviation from the ideal ionic charges if the F and the O1 (or O2) positions are interchanged. , Single-Crystal Raman Spectroscopy Single-crystal Raman spectra were acquired for all crystals. Since all structures are isotypic, Figure shows the spectrum of SmFWO4 as representative of the whole series. The highest frequency peak in the spectrum is located at about 946 cm–1, which correlates to stretching vibrations of the terminal W6+–O2– groups. Stretching vibrations as well as deformation modes relating to the longer edge-connecting W6+–O2– entities are found from 790 down to 500 cm–1, while the bands at lower wavenumbers are assigned to RE 3+–O2–/F– as well as lattice vibrations. Single-crystal Raman spectrum of SmFWO4 as a typical representative of the REFWO4 series with RE = Y, Sm–Lu. Luminescence Spectroscopy YFWO4 and GdFWO4 were activated with nominally 1 mol % Eu3+ and Tb3+, respectively, to investigate their luminescence properties. The excitation and emission spectra at T = 80 K are depicted in Figures and . Both compounds show the typical 4f6 ← 4f6 of Eu3+ or 4f8 ← 4f8 transitions of Tb3+ in their excitation spectra, respectively. In addition, broad excitation bands are observable in the UV range that probably stem from a W6+ ← O2– ligand-to-metal charge transfer (LMCT) transition (eventually with overlapping 4f75d1 ← 4f8 transitions in the case of the Tb3+-activated compounds that cannot be fully excluded in that spectral range). At 80 K, the intensity of those bands is comparably low, which indicates a limited indirect crossover via these states. Excitation (top) and emission spectra (middle) of YFWO4:Eu3+ (left column, orange graphs) and GdFWO4:Eu3+ (right column, red graphs) at T = 80 K. Decay curves of the 5D0-based luminescence at T = 80 K are shown at the bottom. Excitation (top) and emission spectra (middle) of YFWO4:Tb3+ (left column, bright green graphs) and GdFWO4:Tb3+ (right column, dark green graphs) at T = 80 K. Decay curves of the 5D4-based luminescence at T = 80 K are shown at the bottom. Only a single line for the 5D0 ↔ 7F0 transition is observed, which indicates only one crystallographically independent RE 3+ site in the regarded fluoride tungstates, in agreement with the implications from the single crystal structure data. The emission spectra of the Eu3+-activated fluoride tungstates are dominated by transitions from the 5D0 level, even upon excitation into the 5L6 level at 396 nm. This is surprising given the correspondingly low cutoff phonon energy of 946 cm–1 (see Figure ) that would formally imply rather slow nonradiative decay from the 5D1 level (ΔE = 1750 cm–1) according to the energy gap law. In fact, the total decay time of the 5D1 level in these hosts is merely between 7 and 8 μs. This is to be compared to, e.g., YAl3[BO3]4:Eu3+ with a higher cutoff phonon energy of around 1400 cm–1 but yet a corresponding decay time of the 5D1 level of almost 18 μs, in contrast to the expectations of the energy gap law. The observation of dominant 5D0-based luminescence indicates that nonradiative multiphonon relaxation in the fluoride tungstate is unusually fast, which will be investigated in more detail in a future dedicated study. The decay time of τ = 0.77–0.79 ms of the 5D0 level (single exponential decay) at T = 80 K is in line with that low cutoff phonon energy but unusually short and indicates a strongly induced electric dipolar character of the respective transition. This observation also agrees with the strong hypersensitive 5D0 → 7F2 transition at 613 nm that is particularly affected by this admixture according to Judd–Ofelt theory. Again, the comparison to YAl3[BO3]4:Eu3+ is insightful here, as the corresponding decay time of the 5D0 level in that compound is longer with τ = 1.35 ms despite its higher cutoff phonon energy. In the case of the Tb3+-activated fluoride tungstates, the emission spectra show dominant, typical green luminescence from the energetically isolated 5D4 level of Tb3+ with a similarly short decay time of τ = 0.75 ms at T = 80 K despite the low maximum vibrational energy. To compare, the respective decay time in the huntite-type borate YAl3[BO3]4:Tb3+ at T = 80 K is around τ = 2.0 ms, again in contrast to expectations according to the energy gap law. This strong difference also implies a strong admixture of the LMCT state into the 4f8 spin–orbit levels of Tb3+ in the regarded fluoride tungstates. Interestingly, excitation into the higher energetic 5D3 level reveals radiative 5D3 → 7F J (J = 6···0) transitions in the blue spectral range. This is to be expected given the very large energy gap of around ΔE = 5700 cm–1 between the 5D3 and 5D4 levels compared to the maximum phonon energy of 946 cm–1 (see Figure ) that basically limits nonradiative multiphonon relaxation. Yet, the relative intensity of the 5D3-based emission below 500 nm is unusually small given those boundary conditions. One possible reason could be cross relaxation of the 5D3 level, which can be, however, limited at low Tb3+ fractions. The closest RE–RE distances in the regarded fluoride tungstates are 375–385 pm (RE = Y) or 387–393 pm (RE = Gd), which makes such an energy transfer process probable in principle. However, such energy transfer processes should lead to multiexponential decays, , which is not observed in this sample probing the time-resolved luminescence of the 5D3 level with a total decay time of τ = 0.13 ms at T = 80 K. Like in the case of Eu3+, the corresponding decay time of the 5D3 level in YAl3[BO3]4:Tb3+ at T = 80 K is τ = 0.03 ms, which is surprisingly similar despite the lower number of around p = 4 required phonon modes compared to p = 6 for REFWO4:Tb3+ (RE = Y, Gd). Thus, also for Tb3+, an unusually fast nonradiative decay based on admixture of the energetically close LMCT state may be anticipated that will be investigated in more detail in a future study. Measurements of Magnetic Properties The shielded nature of the 4f orbitals generally limits exchange interactions and thus typically leads to ordering temperatures of well below 10 K in the case of rare-earth compounds. Together with the shortest distances between the solely magnetically active cations Gd3+ in the investigated sample of GdFWO4 being 386 pm, magnetic interactions between them are highly unlikely. Thus, the sample displays almost ideal Curie–Weiss behavior throughout the entire temperature range (see Figure ). The respective fit according to χ = C/(T – θ) revealed a Curie constant of C = 7.53(1) K and θ = −0.61(1) K, which results in a calculated magnetic moment of 7.76(1) μB. This is about 2% slightly smaller than the theoretical one of 7.94 for Gd3+ cations, which can probably be explained by a slight amount of amorphous, nonmagnetic byproduct, such as SiO2 from the reaction container. Molar magnetic susceptibility (χmol, blue curve) and inverse molar magnetic susceptibility (1/χmol, red curve) of GdFWO4. Conclusion In this publication, the discovery of the novel rare-earth metal fluoride oxidotungstates with the composition REFWO4 for the smaller elements RE = Y, Sm–Lu is reported. After countless synthesis attempts, the utilization of cesium bromide as a fluxing agent proved to be successful in producing this class of compound. Besides the crystal structure determination, the luminescence properties of Eu3+- and Tb3+-doped yttrium and gadolinium representatives were investigated. In all cases, the typical W6+ ← O2– ligand-to-metal charge transfer is visible with a maximum of 285 nm, which is at wavelengths usually expected for hexavalent tungsten in a tetrahedral coordination. Experimental Section Syntheses 0.25 mmol of the rare-earth metal oxides RE 2O3, namely Y2O3 (99.9%, ChemPur, Karlsruhe, Germany), Sm2O3 (99.9%, ChemPur, Karlsruhe, Germany), Eu2O3 (99.99%, ChemPur, Karlsruhe, Germany), Gd2O3 (99.99%, Aldrich, Darmstadt, Germany), Dy2O3 (99.9%, ChemPur, Karlsruhe, Germany), Ho2O3 (99.9%, ChemPur, Karlsruhe, Germany), Er2O3 (99.999%, ChemPur, Karlsruhe, Germany), Tm2O3 (99.9%, ChemPur, Karlsruhe, Germany), Yb2O3 (99.99%, ChemPur, Karlsruhe, Germany), Lu2O3 (99.9%, ChemPur, Karlsruhe, Germany) and the same amount of rare-earth metal fluorides REF3, YF3 (99.9%, ChemPur, Karlsruhe, Germany), SmF3 (99.9%, Heraeus, Hanau, Germany), EuF3 (99.9%, ChemPur, Karlsruhe, Germany), GdF3 (99.99%, Aldrich, Darmstadt, Germany), TbF3 (99.9%, ChemPur, Karlsruhe, Germany), DyF3 (99.9%, ChemPur, Karlsruhe, Germany), HoF3 (99%, ChemPur, Karlsruhe, Germany), ErF3 (99.9%, ChemPur, Karlsruhe, Germany), TmF3 (99.9%, ChemPur, Karlsruhe, Germany), YbF3 (99.9%, ChemPur, Karlsruhe, Germany), LuF3: (99.9%, ChemPur, Karlsruhe, Germany), as well as 0.75 mmol tungsten trioxide WO3 (99.9%, Aldrich, Darmstadt, Germany) were heated together with 800 mg CsBr (99%, abcr, Karlsruhe, Germany) as flux in fused and graphitized, evacuated silica ampules for 7 days at 700 °C. Due to the commercial unavailability of Tb2O3, a 3:2 mixture of Tb4O7 (99.9%, Onyxmet, Olsztyn, Poland) and 11 mg Tb (99.9%, ChemPur, Karlsruhe, Germany) was used for the in situ generation of Tb2O3. The furnace was cooled down in 2 days to 630 °C and then in 1 day to room temperature. The ampules were opened and the contained bulk product, which remains stable to atmospheric influences, was washed with demineralized water and was dried at 50 °C. Finally, coarse single crystals, exhibiting the color of the respective trivalent rare-earth metal cation (colorless for RE = Y, Eu, Gd, Tb, Dy, Tm, Yb, Lu; pale yellow for RE = Sm; yellow for RE = Ho; and pink for RE = Er), were selected for X-ray diffraction and Raman spectroscopy. For the synthesis of the activated samples of YFWO4 and GdFWO4, double the amount of the initial reaction mixture was used with an activation grade of about 1% Eu2O3 or Tb4O7, respectively. Single Crystal Structure Determination Single crystal data sets of the REFWO4 representatives were collected with the help of a StadiVari diffractometer (Stoe & Cie., Darmstadt, Germany) equipped with a microfocus source emitting Ag–Kα radiation (λ = 56.093 pm) and a Pilatus 200K detector (Dectris, Baden, Switzerland). Background, polarizations, and Lorentz factor corrections as well as scaling of the reflection intensities were performed by the program STOE LANA. Structure solutions and refinements were carried out with the program package SHELX-2019 , (65 refined parameters for all crystals). The compounds crystallize isotypically in the triclinic space group P1̅ with two formula units per unit cell. For some of the structure refinements, a high residual electron density is observed around the tungsten and/or the rare-earth metal atoms in the structure. This is mostly due to the rather high diffraction angle, which produces these artifacts. However, due to refining very strong diffracting atoms (W and RE) next to rather weak ones (O and F), the high angle is needed in order to gain enough information on the latter ones for adequate positional and anisotropic refinement. Cutting those angles to significantly smaller ones would result in less residual electron density; however, it would also result in the loss of the ability to refine oxygen and fluorine anisotropically. Further information on the crystallographic data can be found in Tables – as well as from the joint CCDC/FIZ-Karlsruhe online deposition service: https://www.ccdc.cam.ac.uk/structures/? by quoting the deposition numbers CSD-2456963 for YFWO4, CSD-2456971 for SmFWO4, CSD-2456969 for EuFWO4, CSD-2456970 for GdFWO4, CSD-2456964 for TbFWO4, CSD-2456973 for DyFWO4, CSD-2456966 for HoFWO4, CSD-2456967 for ErFWO4, CSD-2456968 for TmFWO4, CSD-2456972 for YbFWO4, CSD-2456965 for LuFWO4. 3Crystallographic Data of the REFWO4 Representatives with RE = Y, Sm, Eu, and GdCrystallographic dataYFWO4 SmFWO4 EuFWO4 GdFWO4 a/pm467.26(2)468.55(3)467.88(1)467.33(2) b/pm599.66(3)617.35(4)613.88(1)610.95(3) c/pm683.55(3)694.31(4)692.24(2)691.19(4)α/°88.879(4)89.497(5)89.367(2)89.271(4)β/°82.256(4)83.149(5)83.030(2)82.955(4)γ/°75.227(4)74.839(5)74.892(2)74.940(4)ρc/g·cm–1 6.4397.2017.3027.449 V m/cm3·mol–1 55.25057.93657.35856.936 F(000)308354356358Measuring range ±h; ±k; ±l 7; –7/9; 117; 10; –9/117; –10/8; 117; 10; –10/112θmax/°55.7156.7455.7255.71μ/mm–1 25.4024.1024.8725.62Number of coll./unique reflections8176/168211047/19599629/18488363/1784 R int/R σ 0.018/0.0180.041/0.0450.023/0.0150.020/0.019 R 1 for n refl. with |F 0| ≥ 4σo(F 0)0.016; n = 16220.022; n = 16090.022; n = 18020.020; n = 1690 R 1/wR 2 for all reflections0.017/0.0380.030/0.0490.022/0.0540.021/0.050 GooF 1.0840.9451.0871.079Residual electron density ρmax/ρmin/10–6 e –·pm–3 1.93/–1.853.11/–3.232.25/–3.922.47/–2.44 Crystallographic Data of the REFWO4 Representatives with RE = Y, Sm, Eu, and Gd 4Crystallographic Data of the REFWO4 Representatives with RE = Tb, Dy, Ho, and ErCrystallographic dataTbFWO4 DyFWO4 HoFWO4 ErFWO4 a/pm467.19(1)466.78(3)467.33(2)467.59(2) b/pm607.98(2)603.45(3)600.78(3)591.17(2) c/pm688.01(2)686.08(4)684.20(3)682.19(3)α/°89.028(2)89.000(4)88.898(3)88.836(3)β/°82.606(2)82.482(4)82.283(3)82.127(3)γ/°74.935(2)75.096(4)75.183(3)75.328(3)ρc/g·cm–1 7.5577.7037.7857.899 V m/cm3·mol–1 56.34055.74155.46454.958 F(000)360362364366Measuring range ±h; ±k; ±l 7; –6/10; 117; –10/9; –10/117; –10/8; 11–6/7; 9; 112θmax/°55.7255.7255.7355.72μ/mm–1 26.4827.3928.1229.15Number of coll./unique reflections10409/181211906/179111621/178010009/1758 R int/R σ 0.026/0.0200.019/0.0170.032/0.0220.018/0.013 R 1 for n refl. with |F 0| ≥ 4σo(F 0)0.022; n = 16630.013; n = 16040.021; n = 16310.015; n = 1699 R 1/wR 2 for all reflections0.025/0.0560.016/0.0260.024/0.0500.016/0.037 GooF 0.9981.0041.1021.089Residual electron density ρmax/ρmin/10–6 e –·pm–3 3.63/–3.241.46/–1.372.43/–2.361.41/–1.46 Crystallographic Data of the REFWO4 Representatives with RE = Tb, Dy, Ho, and Er 5Crystallographic Data of the REFWO4 Representatives with RE = Tm, Yb, and LuCrystallographic dataTmFWO4 YbFWO4 LuFWO4 a/pm468.76(2)468.96(2)470.61(2) b/pm594.26(3)590.99(3)588.58(3) c/pm679.78(3)677.08(3)675.93(3)α/°88.778(4)88.777(4)88.750(4)β/°81.820(3)81.652(4)81.411(4)γ/°75.337(3)75.498(4)75.360(4)ρc/g·cm–1 7.9828.1288.183 V m/cm3·mol–1 54.59454.11853.992 F(000)368370372Measuring range ±h; ±k; ±l 7; 9; 117; –9/8; 11–7/5; 9; 112θmax/°55.7255.7155.73μ/mm–1 30.0031.0531.90Number of coll./unique reflections9549/174710434/173611814/1736 R int/R σ 0.027/0.0170.027/0.0240.039/0.025 R 1 for n refl. with |F 0| ≥ 4σo(F 0)0.022; n = 16870.017; n = 15160.024; n = 1586 R 1/wR 2 for all reflections0.023/0.0560.021/0.0360.028/0.060 GooF 1.1660.9661.083Residual electron density ρmax/ρmin/10–6 e –·pm–3 3.34/–4.151.49/–1.764.25/–3.53 Crystallographic Data of the REFWO4 Representatives with RE = Tm, Yb, and Lu X-ray Powder Diffractometry Powder X-ray data were collected for all compounds on a STADI-P powder diffractometer (Stoe & Cie., Darmstadt, Germany) equipped with a MYTHEN-1K detector (Dectris, Baden, Switzerland), utilizing monochromatized Cu–Kα1 radiation (λ = 154.056 pm). The samples were recorded in transmission mode upon placing the bulk product on appropriate adhesive tape. In most cases, the bulk products could not be confirmed to be single phase due to the reaction in silica ampules with rare-earth metal fluorides as reactants, which are known to attack the container walls, even if they are graphitized. A LeBail-Fit, performed with the program package FullProf, of YFWO4 as a representative for the whole series, is depicted in Figure . The rather ragged difference curve (blue line) can be attributed to the uneven texture of the crystallites. LeBail fit of the powder pattern of YFWO4. Raman Spectroscopy Single-crystal Raman spectra of the title compounds were collected with the help of a Horiba XploRa spectrometer (Kyoto, Japan), utilizing a red LASER with a wavelength of λ = 632 nm. Luminescence Spectroscopy Photoluminescence spectra were acquired with an FLS1000 photoluminescence spectrometer from Edinburgh Instruments. It was equipped with a 450 W Xe arc lamp for excitation, double grating excitation, and emission monochromators in Czerny-Turner configuration, and a thermoelectrically cooled (−20 °C) photomultiplier tube PMT-980 (Hamamatsu). Emission spectra were corrected with respect to the grating efficiency and PMT sensitivity, while excitation spectra were additionally corrected with respect to the lamp intensity. Time-resolved luminescence was probed with an Edinburgh Instruments μF2 μs flash lamp (60 W pulsed Xe arc lamp) with adjustable trigger frequency (0.1 Hz···1000 Hz) and temporal pulse width of Δτ ≈ 2 μs using single-photon multichannel scaling (MCS) as the detection mode. Low-temperature measurements were performed with a Linkam Scientific THMS600 temperature cell with an accuracy of ±0.1 °C in the temperature range between −196 °C (liquid nitrogen) and room temperature regarded within this work. The signal was coupled to the spectrometer with optical fiber bundles from the temperature cell. Measurements of Magnetic Properties 54 mg of microcrystalline GdFWO4 was placed in a gelatin capsule and attached to the sample holder of a vibrating sample magnetometer for measuring the magnetization M(T) in a magnetic property measurement system (MPMS3, Quantum Design, San Diego, CA, USA). The sample was examined in the temperature range between 5 and 300 K in a homogeneous magnetic field of 500 Oe to calculate the molar (χmol) and the inverse molar susceptibility (1/χmol) of the aforementioned sample. Diamagnetic corrections were performed according to Bain and Berry.