LiMPtTl (M = Ti, Zr) Heusler alloys for high-performance energy harvesting: a DFT study Authors: Ramesh Sharma, Ali B M Ali, Jisha Annie Abraham, Jaya Madan, Nikhil Shrivastav, Sabirov Sardor, Mirjalol Ismoilov, F F Al-Harbi, Awatif Alshamari Published: 2026 ABSTRACT AbstractThe current study explores the electronic, thermodynamic, elastic, optical, and thermoelectric properties of the quaternary Heusler alloys LiMPtTl (M = Ti, Zr) using the full-potential linearized augmented plane wave method within the framework of density functional theory, along with semiclassical Boltzmann transport theory. Band structure and density of states calculations indicate semiconducting behavior with indirect band gaps of 0.84 eV for LiTiPtTl and 0.99 eV for LiZrPtTl. Calculations of formation energies, elastic constants, and temperature-dependent thermodynamic properties indicate structural stability, mechanical robustness, and overall stability, while also reflecting anisotropic properties. Optical spectra indicate strong dielectric behavior in the low-energy regime (~ 2 eV), followed by a gradual decrease in the higher energy range. Strong ultraviolet reflectivity indicates potential applications in UV-protective coatings, while strong optical conductivity in the visible region indicates potential applications in solar energy conversion. Transport calculations indicate an increasing power factor with temperature, indicating their potential applications in high-temperature thermoelectric devices. The lattice thermal conductivity calculated from the Slack model predicts very low values of 0.68 W m⁻¹ K⁻¹ for LiTiPtTl and 1.15 W m⁻¹ K⁻¹ for LiZrPtTl at 300 K. The Seebeck coefficients for both compounds are very high at room temperature: 1349.2 and 1890 µV K⁻¹. LiTiPtTl attains a peak figure of merit (ZT) of 0.73 at 1200 K, surpassing many reported quaternary Heusler systems in both magnitude and thermal stability. Owing to the scarcity of prior studies on these materials, these findings provide a useful platform for future theoretical and experimental exploration. This issue makes this investigation useful as future research is necessary due to a lack of previous studies.Supplementary InformationThe online version contains supplementary material available at 10.1038/s41598-026-56145-w.Keywords: Quaternary Heusler alloys; LiMPtTl (M = Ti, Zr); Optoelectronic properties; Thermoelectric performance; Seebeck coefficient; Power factor; Lattice thermal conductivity; Energy harvestingSubject terms: Materials science, Physics Introduction The pace of technological development and the requirements of modern life have resulted in a substantial increase in energy consumption worldwide, making it a challenge to produce sustainable energy. Under these conditions, there is a great need for energy solutions that are reliable, safe, and easy to implement. Thermoelectric technology, based on the Seebeck effect, has these advantages and does not produce dangerous emissions during operation. Therefore, there has been great interest in finding environmentally friendly and efficient energy sources to solve the current energy crisis. Thermoelectric energy conversion is one of the promising methods for the direct conversion of waste heat into usable electrical power. Heusler alloys were first reported by Friedrich Heusler in early 20th century (1903)1. He experimented with alloys like Cu2MnAl and found that even though the constituent elements were non-magnetic in nature, the alloy exhibits ferromagnetic behaviour. Heusler alloys have been classified into full Heusler (), half Heusler ( XYZ) and quarternary Heusler (). Full Heusler alloys () have a highly ordered cubic structure with all lattice sites filled and usually show metallic or half metallic behaviour useful in spintronics. Half Heusler alloys ( XYZ) have structure, where one of the four interpenetrating fcc sublatttices is vacant, making them to behave as semicondutcors with tuneable band gaps and suitable for themoelectric applications. Quaternary Heusler alloys () contain four different elements in an ordered structure, allowing precise tuning of electronic, magnetic and thermoelectric properties2–5. As Thermoelectric Modules (TEMs), made of TE materials, do not produce any pollutants during operation, this method is considered environmentally friendly for future energy applications6. The performance of a thermoelectric material is measured by the dimensionless Figure of merit (ZT), given by: where S is the Seebeck coefficient, σ is electrical conductivity, and T is the absolute temperature. The symbols κe and κl stand for electronic and lattice thermal conductivity, respectively7. Though many research scholars and scientists are actively trying and working hard towards finding more materials with a good value of ZT, only a few materials have demonstrated a value of 1 and ZT at room temperature8–10. In the present-day scenario, the contemporary problem for modern research is how to solve the problem of the development of materials that would not only have good mechanical and electrical properties but would also be useful for the practical application of TE. It is within this backdrop that Heusler alloys have surfaced as a hopeful candidate. Not only have they produced materials with good mechanical stability, but they have also become quite useful for the practical application of the devices/host materials11–13. Nevertheless, by containing an appropriate quantity of electropositive elements, for instance, lithium, and by following the 18 valence electrons rule, the vacant positions in the HH or FH structures can be utilized for creating a new class of materials that is referred to as quaternary Heusler compounds. It is worth pointing out that some of the HH and FH structures were found to attract considerable attention due to their unique electronic and magnetic properties, which can potentially lead to their applications in various fields including topological devices, spintronics, ferromagnetism, etc., which is where the subject of superconductivity is moving towards14–16. It has been stressed that the efficient thermoelectric materials were required to feature a small semiconductor gap together with phonon glass-electron crystal property17. Such good properties can be perfectly seen with regard to the alloys of Heusler materials. Such good properties have to be used for thermoelectric devices. The Heusler alloys received immense attention due to their non-toxic properties, thermodynamic, and mechanical stability, along with their semiconductor characteristics, which are available at low cost18–23. While thermoelectric materials have abundant and affordable elements available, significantly, several Heusler alloys have shown good thermoelectric properties with abundant and affordable elements available on the Earth’s crust material24. Half-Heusler (HH) materials composed of Ti, Hf, and Zr have been found to be of significant interest to researchers due to their diverse range of physical properties and applicability in thermoelectric devices25,26. These materials have attracted considerable research interest over the past few years, and it has been found that they can exhibit notable mechanical properties along with thermoelectric properties27,28. Research on both n-type and p-type HH materials has found promising Figure of merit at high temperature ranges, i.e., around 0.8 to 1.0529. Among the Sb-based HH materials, several have been found to exhibit significant Figure of merit, i.e., higher than unity30,31. Among these materials, LaPtSb has shown promising performance for thermoelectric energy conversion, with a Figure of merit near 2.2 under near-room-temperature conditions32,33. In recent studies, several Heusler alloys have been explored using a wide variety of experimental techniques and density functional theory studies, suggesting good mechanical stability coupled with good thermoelectric performance, largely attributed to the low lattice thermal conductivity inherent in Heusler alloys34. The field of quaternary Heusler materials with multifunctional characteristics has been explored theoretically to assess their potential for existing and future technologies35. It is well established that quaternary Heusler compounds typically exhibit lattice constants in the range of ~ 5.8–6.5 Å and relatively high bulk moduli, indicating strong structural rigidity and mechanical stability1,36. For example, Zr-based quaternary Heusler alloys have been reported to possess bulk moduli in the range of ~ 120–200 GPa, confirming their high resistance to compression and structural robustness1. Similarly, other Li-based Heusler systems show comparable formation energies and follow the general trend of enhanced stability for negative formation energies, consistent with thermodynamically stable phases36. The results confirm that their structural parameters are in good agreement with previously reported stable Heusler and quaternary Heusler alloys, thereby supporting their mechanical and thermodynamic stability. It is interesting to note that a quaternary Heusler compound, CrVNbZn, has been theoretically explored using density functional theory methods, yielding good electronic, magnetic, and thermoelectric properties, with a peak ZT of 0.79 over a temperature range of 260–480 K37. A superior thermoelectric material, with a figure of merit ZT = 1.22, has also been reported for the quaternary Heusler alloy compound NaHfCoGe, thereby highlighting its potential for application as a thermoelectric material38. Apart from these compounds, a number of other Li-based quaternary Heusler compounds, such as LiHfCoX (X = Ge, Sn), LiNbCoX (X = Al, Ga), LiScPdPb, LiTiCoZ (Z = Si, Ge), and LiTiPdZ (Z = Al, Ga, In)39–41, were also investigated for their potential for application as thermoelectric materials. Li-based quaternary Heusler alloys such as LiTiPtZ (Z = Al, Ga, In) have been reported to exhibit semiconducting band gaps and promising thermoelectric performance42. Similarly, Fe-based quaternary Heusler compounds like FeCrTiSb demonstrate high thermoelectric efficiency along with favorable electronic and optical properties43. In addition, other quaternary systems such as CoFeYGe (Y = Ti, Cr) show good transport characteristics and moderate thermoelectric performance44. A literature survey shows that LiMPtTl, where M = Ti, Zr, are yet to be explored both theoretically and experimentally, thus prompting us to investigate their ground state structural parameters, electronic, elastic, and optical properties, along with their potential for application as thermoelectric materials. Computational approaches The structural, electronic, dynamical, thermodynamic, elastic, optical, and transport properties of quaternary Heusler compounds LiMPtTl (M = Ti, Zr) were studied within the framework of density functional theory implemented in the WIEN2k45 simulation package using a full-potential linearized augmented plane wave (FP-LAPW) approach. This fully relativistic method is particularly apt to deal with complex crystal geometries and chemical bonds, providing an adequate description of electronic properties. To describe the exchange–correlation effects, the generalized gradient approximation (GGA) of Perdew–Burke–Ernzerhof (PBE)46 was applied, this functional representing a good compromise between computational cost and accuracy for solid-state systems. To take advantage of improved band gap values, the Tran–Blaha modified Becke–Johnson47 potential was further adopted, since it has become evident that these functional yields semiconductor and insulator electronic structures closer to experiment. The relativistic effects ensuing from the heavier atoms, Pt and Tl, were treated by including spin–orbit effects48 via the second-variational scheme provided by WIEN2k. Brillouin zone sampling49 was performed using a 17 × 17 × 17 Monkhorst–Pack mesh in reciprocal space. The used muffin-tin radii were 2.0 a.u. for Li and Ti/Zr, 2.25 a.u. for Pt, and 2.0 a.u. for the rest, with the following basis set parameter values. The chosen muffin-tin radii were 2.0 a.u. for Li and Ti/Zr, 2.25 a.u. for Pt, and 2.0 a.u. for the remaining atoms, while the basis-set parameters were set to RMTKmax=7 and Gmax =12, ensuring proper convergence of the potential and wavefunctions. A separation energy of − 7.0 Ry distinguished core from valence states. Self-consistent calculations were continued until the total energy and charge converged to 10− 4 Ry and 10− 4 e, respectively. The thermoelectric transport coefficients were calculated by using the BoltzTraP code50 under the empirical Boltzmann transport theory, applying a constant relaxation time and a rigid band approach approximation. A dense mesh of around 1,00,000 k-points was used during calculations for the transport integral with a chosen carrier relaxation time of 10− 14 s, as such, was assumed, as is generally adopted in such systems of intermetallic compounds. However, results may be further refined in any further studies involving temperature-dependent relaxation times, obtained from electron-phonon couplings by tools such as EPW, to arrive at higher precision calculations. Results and discussion Structural & thermodynamic stability The quaternary Heusler compounds LiMPtTl (M = Ti, Zr) possess an equiatomic composition (1:1:1:1) and form a face-centered cubic structure belonging to the F-43 m space group. Their electronic behavior is closely linked to the specific atomic ordering, which may occur in three possible configurations commonly referred to as type-1, type-2, and type-3 arrangements and their Wyckoff positions are listed in Table 1 (see Fig. 1(a-c)). To identify the energetically preferred configuration and evaluate the equilibrium structural parameters, such as lattice constant (a), bulk modulus (B₀), and minimum total energy (E₀), a series of volume optimization calculations were performed for each configuration. Table 1Atomic configurations of QH LiMPtTl (M = Ti, Zr) alloys in type 1, 2, and 3.ElementsPhase 1Phase 2Phase 3Li0.75,0.75,0.750.5, 0.5, 0.50.75,0.75,0.75M=Ti/Zr0.25,0.25,0.250.75,0.75,0.750,0,0Pt0.5, 0.5, 0.50.25,0.25,0.250.25,0.25,0.25Tl0,0,00,0,00.5, 0.5, 0.5 Atomic configurations of QH LiMPtTl (M = Ti, Zr) alloys in type 1, 2, and 3. Crystal structure for three types of cubic structure for QH LiMPtTl (M = Ti, Zr) compounds using GGA. The total energy versus volume data were fitted using the third-order Birch–Murnaghan51 equation of state: where is the equilibrium energy, is the equilibrium volume, is the bulk modulus, and is its pressure derivative. Figure 2(a, b) show the variation of total energy with unit-cell volume for LiTiPtTl and LiZrPtTl, respectively. In both materials, the type-3 configuration shows the minimum energy, hence it is the most stable phase. The calculated bulk modulus has a value larger than 100 GPa in each case, which indicates that these compounds have good mechanical stability and strong resistance against external compression. The feasibility of experimental preparation of a given material can be estimated by using a formula to compute the material’s formation energy (Ef), which is given by: Total energy as a function of volume for three types of cubic structure for QH LiMPtTl (M = Ti, Zr) compounds using GGA. Here and represent the ground-state energies of the quaternary Heusler alloy LiMPtTl (M = Ti, Zr) and its constituent elements, respectively, and Nis the total number of atoms in the unit cell. For both alloys studied, the calculated formation energies are negative, indicating that the compounds are thermodynamically favorable to be stable (Table 2). This implies that their experimental synthesis may be feasible, making LiMPtTl (M = Ti, Zr) alloys promising candidates for further investigation and potential applications. Table 2Calculated ground-state structural parameters of QH LiMPtTl (M = Ti, Zr) alloys.AlloyPhasea(Å)V0(a.u.3)B0(GPa)B(GPa)E0(Ry)Ec(eV/atom)Ef(eV/atom)LiTiPtTlPhase 16.46456.0999.956.16-79194.0581591.95-0.822Phase 26.47457.46103.905.66-79193.994429Phase 36.44451.25117.025.75-79194.077278Ref.6.1828LiZrPtTlPhase 16.70508.8594.075.17-84684.8720322.20-0.743Phase 26.62491.07102.965.61-84684.813088Phase 36.60485.40117.024.89-84684.912129Ref.6.4239 Calculated ground-state structural parameters of QH LiMPtTl (M = Ti, Zr) alloys. The cohesive energy () quantifies the strength of bonding between atoms in a material and serves as a measure of its structural stability52,53. It can be expressed as: where N is the total number of atoms in the unit cell, is the total energy of the isolated constituent atoms, and is the total ground-state energy of the quaternary Heusler alloy LiMPtTl (M = Ti, Zr). Strong interatomic bonding and structural stability of the alloys are confirmed by the computed cohesive energies, which are both positive and significant for LiTiPtTl and LiZrPtTl. These results, in addition to the negative formation energies, show that the alloys are possible for experimental synthesis and thermodynamically favorable, making those excellent candidates for additional research. Mechanical properties Understanding the strength and mechanical stability of a crystal requires knowledge of its elastic constants. The IRelast code54, which calculates the stress-strain behavior of a crystal under minor deformations, was employed to calculate the elastic constants and the corresponding mechanical properties of LiTiPtTl and LiZrPtTl. Three independent elastic constants, namely C11, C12, and C44, are sufficient to describe the elastic behavior of cubic crystals. The elastic constants are calculated by keeping the volume constant and applying small strains at zero pressure. The mechanical stability of a crystal is determined by the Born-Huang criteria55: Both LiTiPtTl and LiZrPtTl satisfy these conditions (Table 3), confirming their mechanical stability. Table 3Calculated elastic constants and derived mechanical parameters of QH LiMPtTl (M = Ti, Zr).Mechanical parametersLiTiPtTlLiZrPtTlC11 (GPa)149.4690156.3666C12 (GPa)101.036597.83C44 (GPa)102.272590.93B (GPa)117.180117.34S (GPa)57.86157.80Y (GPa)149.050148.96Pugh’s ratio (B/G)2.022.03Poisson’s ratio (ʋ)0.2880.288(A)4.223.10Cp-1.2366.9ʋt(ms-1)2264.752243.2ʋl(ms-1)4150.454113.81ʋm(ms-1)2525.872501.96θD294.104284.322Tm1436.36171477.12 Calculated elastic constants and derived mechanical parameters of QH LiMPtTl (M = Ti, Zr). To gain further insight, the bulk modulus ( B), shear modulus ( S), and Young’s modulus ( E) were calculated using the Voigt–Reuss–Hill (VRH) approximation. For cubic crystals, the Voigt and Reuss bounds are expressed as56–58: Voigt approximations : Reuss approximations: The Hill average is then obtained as the arithmetic mean of the Voigt and Reuss bounds: Finally, Young’s modulus Eand Poisson’s ratio are calculated as59: In this case, B is the resistance to volume compression, G is the resistance to shape deformation, while Equantifies the resistance to elongation or contraction due to tensile stress60,61. The values of the moduli calculated for bulk (B), shear (S), and Young’s (E) moduli (Table 3) indicate that LiTiPtTl has slightly higher values than LiZrPtTl, meaning that it is more resistant to volume compression and shape deformation. LiZrPtTl, being less resistant, is relatively more flexible and thus suitable for use in applications where mechanical flexibility is desired. Calculated elastic properties (B, G, E, B/G, and ν) of LiMPtTl (M = Ti, Zr) are compared with reported half-Heusler and quaternary Heusler compounds in Supplementary Table S1. A material’s relative brittleness and ductility can be determined using Pugh’s ratio (B/G), where a ratio of 1.75 indicates ductility62. LiTiPtTl (2.02) and LiZrPtTl (2.03) are both ductile since their ratios are less than this value. Both materials exhibit a combination of covalent and metallic bonding, as indicated by their respective Poisson’s ratios ( v) of 0.288 and 0.288, which are below 0.33. The anisotropy factor A of the elastic properties is a measure of the direction dependence of the elastic properties. A value of 1 is isotropic. The calculated values of 4.22 (LiTiPtTl) and 3.10 (LiZrPtTl) are both anisotropic. The Debye temperature ()63 provides insight into lattice vibrations, phonon contributions, and thermal properties of materials. It can be estimated using the average sound velocity () derived from elastic constants as: where h is Planck’s constant, is Boltzmann’s constant, n is the number of atoms per formula unit, V is the unit cell volume, and is the average sound velocity, calculated from the longitudinal () and transverse () sound velocities: In this case, is the material density, and B and G are the bulk and shear moduli. The Debye temperatures for LiTiPtTl and LiZrPtTl are determined to be 294.10 K and 284.32 K, respectively, using these relations, suggesting that LiTiPtTl has stronger lattice bonding. The relation64 can be used to empirically determine the melting temperature (Tm) from the elastic constants: where is in GPa. Using this formula, the melting points are 1436.36 K for LiTiPtTl and 1477.12 K for LiZrPtTl. The higher and of LiZrPtTl align with its larger elastic moduli, confirming its superior thermal and mechanical stability. Electronic properties The section that follows describes the electronic configuration of the atoms that make up LiTiPtTl and LiZrPtTl, including their valence electrons: Tantalum [5d³ 6s²], Zirconium [4d² 5s²], Platinum [4d⁹ 5s¹], Titanium [3d² 4s²], and Lithium [2s¹]. The aforementioned preparation is necessary to guarantee that both quaternary. It is generally known that Heusler compounds are stable due to the 18-valence electron count (VEC) rule. As per the Slater-Pauling rule11: . The total magnetic moment for both compounds, as per the above equation, which again confirms that both compounds are non-magnetic in nature, as already reported in39,40. The 18-VEC rule also accounts for the band gap between the conduction (anti-bonding) and valence (bonding) bands, which again confirms the semiconducting nature of the compounds65–67. For better understanding, the band structures (BS) of LiTiPtTl and LiZrPtTl are shown in Fig. 3 along with their density of states (DOS), which again shows the atom-wise contributions to the electronic structure. Band structures of the QH LiMPtTl (M = Ti, Zr) compounds with mBJ-GGA at its equilibrium lattice constant. Understanding the electronic characteristics of LiTiPtTl and LiZrPtTl compounds on the high-symmetry path W-L-Γ-X-W-K requires calculations of electronic BS and DOS. Both compounds have indirect band gaps, with the valence band maximum at the Γ point and the conduction band minimum at the X point, according to calculations performed using the GGA-PBE method (Supplementary Fig. S1). They are determined to be semiconductors with band gap values of 0.839 eV for LiTiPtTl and 0.955 eV for LiZrPtTl. The conduction band is occupied from 1.5 to 6.4 eV, and the valence band is filled from − 5.3 eV to the Fermi level (EF). High carrier effective masses are also indicated by the flat Ti/Zr-d and Pt-d bands at EF. The prediction of the band gap is enhanced by employing the TB-mBJ potential (Fig. 4), which maintains the indirect band gap structure with slightly larger gaps of 0.840 eV and 0.994 eV, in agreement with previously reported results39,40. Minor splitting is added around heavy elements (Pt, Tl) by adding SOC (mBJ + SOC) (Supplementary Fig. S1), but the overall band structure and indirect semiconducting character are not affected. Specifically, we now explain that SOC lifts the degeneracy of electronic states and induces band splitting, particularly in the valence bands near high-symmetry points and close to the Fermi level. This splitting can modify the band gap and the density of states, thereby influencing the transport properties. It is also noted that SOC effects are more pronounced in materials containing heavy elements, where relativistic interactions significantly alter band dispersion and carrier dynamics68. Based on the DOS analysis, the VB is dominated by Pt-d, along with Ti/Zr-d and Tl-p orbitals, while the CB is dominated by Ti/Zr-d and Pt-d orbitals. The energy bandgaps obtained from PBE-GGA, mBJ, and mBJ + SOC calculations are listed in (Table 4). These results confirm the suitability of the alloys for optoelectronic and thermoelectric devices and re-emphasize the robustness of the semiconducting character against all methods. Total density of states (TDOS) of the QHH LiMPtTl (M = Ti, Zr) compounds with mBJ-GGA (dash magenta line) at their equilibrium lattice constant. Table 4Calculated energy bandgap and Optical properties of QH LiMPtTl (M = Ti, Zr) by mBJ-GGA.Material propertyLiTiPtTlLiZrPtTlBandgap(eV)PBE-GGA0.8390.955mBJ0.8400.999mBJ+SOC0.7920.962Opticalpropertiesε1 (0)24.3019.80n (0)4.934.45R (0)0.4390.4007 Calculated energy bandgap and Optical properties of QH LiMPtTl (M = Ti, Zr) by mBJ-GGA. Bandgap (eV) Optical properties The conduction band (CB) is mainly caused by Ti/Zr-d and Pt-d states, particularly at 2.5 eV above the Fermi level (EF), according to the total and partial density of states (DOS) of LiTiPtTl and LiZrPtTl (Fig. 5). The valence band (VB) is primarily dominated by Pt-d states, especially at 2.4 eV below . The occupied Pt-d states are found to increase from 7 states/eV in LiTiPtTl to 8 states/eV in LiZrPtTl because of hybridization between Ti/Zr-d and Tl-p orbitals. The band gap in both alloys is primarily dominated by Ti/Zr/Pt-d states, which emphasize the importance of these states in determining the electronic structure. Partial density of states of the QHH LiMPtTl (M = Ti, Zr) compounds with a mBJ-GGA at its equilibrium lattice constant. The charge density maps give a clear visual representation of the distribution of electrons in the crystal structure and help to understand the nature of the chemical bonding. For LiMPtTl (M = Ti, Zr), the charge density distribution in the (110) plane (Fig. 6) indicates a high concentration of electrons between Li-Pt, M-Pt, and Pt-Tl atomic pairs, indicating a high degree of covalent bonding with ionic character. It is also important to note that LiTiPtTl has a slightly more localized electron density distribution, while LiZrPtTl has a slightly more delocalized distribution, which is in line with its slightly larger lattice parameter. Charge density plot along 110 plane of the QHH LiMPtTl (M = Ti, Zr) compounds with a mBJ-GGA at its equilibrium lattice constant. Optical properties The complex dielectric function is composed of two parts and is expressed as where is the real part and is the imaginary part. The real part, , describes the polarization response of the material and indicates the energy regions associated with electronic excitation, polarization, and dispersion of electromagnetic (EM) radiation. The imaginary part, , represents the absorption of EM radiation and is calculated from the momentum matrix elements between occupied and unoccupied electronic states, given by where vand cdenote valence and conduction bands, respectively, are the wave functions, is the unit cell volume, and is the polarization vector of the incident EM field. The real part of the dielectric function is then obtained from using the Kramers–Kronig relation69–71: where denotes the principal value of the integral. From the dielectric function, the refractive index and extinction coefficient are determined as While reflects the dispersion of electromagnetic waves inside the material, quantifies the attenuation arising from optical absorption. The reflectivity, which measures the fraction of incident radiation reflected from the surface, is given by The absorption coefficient is then obtained as where cis the speed of light in vacuum. Finally, the energy-loss function, which is particularly relevant for describing plasmon excitations and the energy loss of fast electrons, is defined as The real part of the dielectric function, ε1 (ω), for LiMPtTl (M = Ti, Zr) is shown in Fig. 7a. The static dielectric constants at zero frequency are 24.30 for LiTiPtTl and 19.80 for LiZrPtTl. The static dielectric constant ε1 (0) can be estimated using the Penn model72, which states that ε1 (0) = 1+((ℏωp)/Eg)2, where ℏωp is the plasma energy and Eg is the fundamental band gap. This equation links the optical properties with the electronic band structure, providing a simplified estimate of the low-energy dielectric function.The values of the static optical parameters are given in Table 4. (a) Complex dielectric function ɛ(ω), (b) Refractive index n(ω), (c) extinction coefficient k (ω), (d) reflectivity coefficient R(ω), (e) absorption coefficient α(ω) and (f) Optical conductivity σ(ω) of QHH LiMPtTl (M = Ti, Zr) compounds versus photon energy using mBJ-GGA. With increasing photon energy, ε1 (ω) increases to reach a maximum polarization of 48.68 and 40.37, then decreases to zero at ≈ 3.21 eV (LiTiPtTl) and 2.68 eV (LiZrPtTl). These values represent zero dispersion points, where the material absorbs electromagnetic radiation most strongly. The negative values of ε1(ω) show that the alloys are reflective of the incoming electromagnetic radiation. The imaginary part, ε2 (ω) (Fig. 7b), describes the energy dissipation of the material. The peak of 42.59 at 1.56 eV for LiTiPtTl is higher than that of 34.06 at 2.29 eV for LiZrPtTl, showing that LiTiPtTl is more efficient at absorbing light. The optical properties, specifically the refractive index and extinction coefficient , describe how a material interacts with electromagnetic radiation in terms of transmission and absorption. As shown in Fig. 7(c, d), for QH LiMPtTl (M = Ti, Zr) alloys, the refractive index closely follows the trend of the real part of the dielectric function , while the extinction coefficient reflects the behavior of the imaginary part . At zero photon energy, values are 4.93 and 4.45 for LiTiPtTl and LiZrPtTl, reaching peak values of 7.18 and 6.56 in the infrared region before decreasing toward the visible and ultraviolet ranges. The extinction coefficient increases in the IR and visible regions, peaking at 3.76 and 3.67 for LiTiPtTl and LiZrPtTl, respectively, and then declines in the UV region. These trends suggest that LiHfRhGe, with a higher , may be more effective as an absorbing material in optoelectronic applications. Optical conductivity reflects the movement of photoexcited electrons and provides insight into bond-breaking processes induced by high-energy electromagnetic radiation. Figure 7(e) shows for QH LiMPtTl (M = Ti, Zr) alloys across photon energies from 0 to 13 eV. The conductivity of both materials is 0 at zero photon energy, and it starts at about 1.4–1.7 eV, which corresponds to the bandgap values determined by DOS analysis and band structure. For LiTiPtTl, the highest values of σ(ω) are 9020.25 Ω-1cm-1 at 1.58 eV, while for LiZrPtTl, they are 10570.00 Ω-1cm-1 at 2.33 eV. The visible region has the largest peak, indicating high photoconductivity, while the first peak is located in the infrared zone. These features demonstrate that both Heusler alloys excellent optical conductivity in the visible spectrum makes them highly promising for usage in solar cell applications. The absorption coefficient α(ω) describes the efficiency of a material in absorbing the incoming electromagnetic radiation at different photon energies. It is also related to the extinction coefficient k(ω). Figure 7(f) plots α(ω) for QH LiMPtTl (M = Ti, Zr) alloys for photon energies ranging from 0 to 10 eV. For QH LiMPtTl (M = Ti, Zr) alloys, α(ω) remains low at low photon energies but increases dramatically around the bandgap, indicating the onset of electronic excitations73,74. Reflectivity represents the fraction of incident electromagnetic radiation reflected from a material’s surface, providing insight into its optical behavior across different energy ranges. Figure 7(g) shows the reflectivity spectra of QH LiMPtTl (M = Ti, Zr) alloys. In the infrared (IR) region, the reflectivity remains relatively low with minor fluctuations, indicating that these alloys are poor reflectors in this range. In contrast, the reflectivity increases significantly in the visible and ultraviolet (UV) regions, reaching peak values of 0.620 at 5.33 eV for LiTiPtTl and 0.634 at 5.78 eV for LiZrPtTl. This suggests that LiMPtTl (M = Ti, Zr) alloys could be effective as coating materials to reduce solar heating in these energy ranges. The energy loss function, , shows the plasmonic characteristics of LiTiPtTl and LiZrPtTl, as depicted in Fig. 7(h). A number of strong peaks appear in the ultraviolet region, representing the plasma resonances with ε1 (ω) ≈ 0 and modest ε2 (ω), and the energy loss is minimal for low photon energies. Due to differences in the electrical structures and valence electron concentrations, the plasmon resonance peaks slightly change when Ti is substituted with Zr. LiMPtTl (M = Ti, Zr) alloys have tunable optical and plasmonic properties, which are extremely sought for next-generation optoelectronic and plasmonic devices, as evidenced by the appearance of several tunable peaks in the ultraviolet range75,76. The static optical parameters are listed in Table 4. Thermoelectric properties Thermoelectricity refers to the direct conversion between thermal and electric energy. In such devices, the temperature difference causes the flow of charge carriers, which in turn leads to the generation of an electric current. The temperature- and chemical potential-dependent thermoelectric properties of QH LiMPtTl (M = Ti, Zr) alloys have been studied to determine their potential for use in thermoelectric devices77–81. Their transport properties are described within the Boltzmann transport theory, which is based on the energy-dependent electrical conductivity tensor, and constant relaxation time approximation (CRTA). CRTA is a method used to calculate transport properties using Boltzmann transport equation by assuming that the electron relaxation time is constant. CRTA ignores detailed scattering and focuses on band structure to estimate transport properties efficiently while rigid band approximation ignores changes in band structure due to doping, limiting their accuracy in materials. The basic relations describing these properties are expressed as follows: Electrical conductivity as a function of temperature ( T) and chemical potential (): Here, is the unit cell volume, and is the Fermi–Dirac distribution function. Electronic thermal conductivity: is used in the estimation of the Seebeck coefficient and represents the contribution of electrons to heat transport. Seebeck coefficient tensor: This equation defines the relationship between the Seebeck coefficient, electrical conductivity, and electronic thermal conductivity. These equations, taken together, provide a means of evaluating transport properties as functions of temperature and chemical potential, including electrical conductivity, the Seebeck coefficient, and electronic thermal conductivity. These are essential for evaluating the efficiency of thermoelectric materials such as LiTiPtTl and LiZrPtTl. The transport properties were calculated using semiclassical Boltzmann transport theory within the constant relaxation time approximation (CRTA), as implemented in the BoltzTraP framework. Within this approach, the electrical conductivity (σ), Seebeck coefficient (S), and electronic thermal conductivity (κₑ) are evaluated as functions of temperature (T) and chemical potential (µ). The calculations were performed by scanning the chemical potential over a wide energy range around the Fermi level to simulate both electron and hole doping conditions. The reported transport coefficients correspond to a range of carrier concentrations, typically spanning from 10¹⁸ to 10²¹ cm⁻³, which are commonly relevant for thermoelectric applications. Unless otherwise specified, the results represent optimized transport behavior at carrier concentrations that maximize the power factor (S²σ). The chemical potential at each temperature was adjusted to reproduce the desired carrier concentration using the rigid-band approximation. This approach assumes that doping shifts the Fermi level without altering the underlying electronic band structure. It should be noted that the CRTA assumes a constant relaxation time (τ), and therefore the calculated electrical conductivity and power factor are expressed in terms of σ/τ. While this approximation enables reliable prediction of trends in transport properties, it may not capture the full scattering physics, particularly at high temperatures or in heavily doped regimes. Furthermore, the rigid-band approximation neglects possible band structure modifications induced by doping, which may introduce deviations in real materials. Despite these limitations, this methodology provides a reasonable first-order estimation of thermoelectric performance and is widely adopted for screening potential thermoelectric materials such as LiTiPtTl and LiZrPtTl. According to Fig. 8(a), the Seebeck coefficient (S) of LiMPtTl (M = Ti, Zr) alloys shows positive values with temperature, indicating that holes are the main charge carriers in both alloys. S increases quickly for both alloys up to 300 K, after which it gradually drops as the temperature rises. We have observed a non-monotonic behavior of Seebeck coefficient in low temperature region i.e., initial increase followed by a decrease can arise from the interplay between carrier concentration and carrier diffusion with temperature. At lower temperatures, the increase in thermally activated carriers enhances the Seebeck coefficient, while at higher temperatures the further increase in carrier concentration leads to stronger bipolar effects and enhanced electrical conductivity, which tends to reduce the Seebeck coefficient82,83. The variation in atomic size between Zr and Ti atoms may be the reason for the noticeable disparity between LiTiPtTl and LiZrPtTl across the whole temperature range. LiTiPtTl and LiZrPtTl have Seebeck coefficients of 220.54 µV/K and 225.11 µV/K at 300 K and 204.06 µV/K and 210.44 µV/K at 1200 K, respectively. It’s interesting to note that LiZrPtTl works better at lower temperatures, whilst LiTiPtTl has a greater S value at temperatures about 700 K. Calculated of (a) Seebeck coefficient, (b) power factor, (c) Electronic thermal conductivity, (d) Thermal electronic conductivity (ke), (e) Lattice thermal conductivity (kL), and (f) Figure of merit (ZT) as a function of the temperature of LiTiPtTl and LiZrPtTl with mBJ-GGA approximation. To achieve improved thermoelectric performance, a high-power factor (PF) is necessary. The temperature dependency of PF for QH LiMPtTl (M = Ti, Zr) alloys is displayed in Fig. 8(b). The presence of a high concentration of Ti/Zr and Pt–d states near the Fermi level in the conduction and valence bands, along with flat bands in the band structure, contributes to the large PF values observed. In both alloys, PF increases with temperature, indicating a promising Figure of merit (ZT), particularly at elevated temperatures. At 1200 K, the maximum PF reaches W··· for LiTiPtTl and W··· for LiZrPtTl. The temperature-dependent electrical conductivity (σ/τ) of QH LiMPtTl (M = Ti, Zr) alloys is plotted in Fig. 8(c). With a constant relaxation period of τ = 0.8 × 1014 s, which is equivalent to the reported values for similar intermetallic compounds, the calculations were performed using the Boltzmann transport theory as implemented in the BoltzTraP code. The electronic structure simulations confirm that these alloys exhibit semiconducting properties, as evidenced by the increase in σ/τ with temperature. At 1200 K, the maximum values reach for LiTiPtTl and for LiZrPtTl. Overall, LiTiPtTl exhibits higher across the entire temperature range, likely due to its larger carrier concentration. Table 5 lists the transport parameters at ambient temperature. Table 5Calculated transport properties of QH LiMPtTl (M = Ti, Zr) by mBJ-GGA.ParametersLiTiPtTlLiZrPtTlTransport properties(300 K)σ/τ1019 (Ωms)-10.9570.752S(µVK)220.54225.11κL (W/mK)0.6831.15κe (1014W/mKs)1.891.50S2σ/τ(1011W/K2ms)4.653.81ZT0.1600.087 Calculated transport properties of QH LiMPtTl (M = Ti, Zr) by mBJ-GGA. Transport properties (300 K) The temperature-dependent electronic thermal conductivity (ke/τ) for QH LiMPtTl (M = Ti, Zr) alloys is displayed in Fig. 8(d). Increased free electron mobility in these semiconducting compounds is indicated by the computed ke/τ values, which rise nearly linearly with temperature. With a few exceptions at higher temperatures, the ke/τ values for both alloys stay constant up to 500 K. The greatest values of ke/τ for LiTiPtTl and LiZrPtTl at 1200 K are 31.75 Wm-1K-1s-1 and 26.92 Wm-1K-1s-1 respectively. The increased mobility of free charge carriers and lattice vibrations, which also increase electrical conductivity, are the causes of the rise in thermal conductivity at higher temperatures. The semiconducting nature of both LiMPtTl alloys is further supported by these observations. The lattice thermal conductivity () of the studied alloys was calculated using the Slack equation84, which is crucial for determining the total thermal conductivity and, in turn, the thermoelectric Figure of merit (ZT) over a wide temperature range: where M is the average atomic mass, is the average sound velocity, δ is the atomic volume, γ is the Grüneisen parameter, T is the absolute temperature, and A is a material constant (~ 3.1 × 10⁻⁶ for many solids) that varies depending on the material. At ambient temperature, the calculated Grüneisen parameter and Debye temperature are 1.37 and 316.98 K for LiTiPtTl, and 2.47 and 297.68 K for LiZrPtTl, respectively. This model provides only an approximate estimation of lattice thermal conductivity, as it relies on empirical parameters and simplifying assumptions regarding phonon scattering and anharmonic effects. Therefore, it should be interpreted as a semi-empirical trend-based model rather than a fully predictive first-principles method. Slack’s model gives only an approximate estimate of lattice thermal conductivity and should be used as a screening tool rather than a fully predictive method, as also noted in related thermoelectric studies85,86. Together with comparable values from the literature, the computed values of κl are shown in Fig. 8(e) and Table 5 and exhibit good consistency enhances thermoelectric qualities at higher temperatures by decreasing with temperature due to increasing phonon dispersion. For all temperatures, LiZrPtTl has a slightly higher than LiTiPtTl. Figure 8(e) indicates that the lattice contribution is important only at low temperatures (below 200 K) and reduces at higher temperatures, thus emphasizing the importance of electronic thermal conductivity at higher temperatures. The thermoelectric performance of a material is quantified by the Figure of merit, ZT, which combines the effects of the Seebeck coefficient ( S), electrical conductivity (), and total thermal conductivity (): The temperature dependence of ZT for LiMPtTl (M = Ti, Zr) alloys is presented in Fig. 8(f). Both alloys display an increasing trend in ZT upto 1200 K, beyond which the trend becomes almost temperature-independent. LiTiPtTl sustains a slightly higher value of ZT over the entire temperature range than LiZrPtTl. At 1200 K, the ZT value reaches 0.73 and 0.70 for LiTiPtTl and LiZrPtTl, respectively. The high and temperature-independent ZT values, especially at higher temperatures, exceed those of similar compounds87, indicating the promise of these alloys for high-temperature thermoelectric applications. Transport properties against of chemical potential () The electronic transport properties of LiMPtTl (M = Ti, Zr) alloys have been investigated as a function of chemical potential () over the range − 2.0 to 2.0 eV at temperatures of 300 K, 700 K, and 1200 K. The results are presented in Fig. 9. Calculated transport coefficients: (a, b) Seebeck coefficient (S), (c, d) Power factor , (e, f) Figure of meritel (g, h) Electrical conductivity (i, j) Electronic thermal conductivity as a function of the Chemical potential of the QHH LiMPtTl (M = Ti, Zr) at 300, 700 and 1200 K. The Seebeck coefficient ( S) as a function of chemical potential is depicted in Fig. 9(a, b). Here, the chemical potential also serves as an indicator of the doping type: negative values correspond to p-type doping, while positive values indicate n-type doping. For both alloys, Sshows a strong dependence on chemical potential and temperature. At room temperature (300 K), LiTiPtTl exhibits a maximum Sof 1437.46 µV/K at 0.38 eV, whereas LiZrPtTl reaches 1708.77 µV/K at 0.45 eV. The slightly lower Seebeck coefficient for LiZrPtTl is attributed to its narrower band gap, which reduces the asymmetry in carrier distribution near the Fermi level. With increasing temperature, decreases for both alloys, reflecting enhanced carrier excitation and reduced energy filtering effects. The power factor (PF = ), a key indicator of thermoelectric efficiency, was calculated across the same chemical potential range (Fig. 9(c, d)). LiTiPtTl achieves a maximum PF of W··· at − 0.046 eV, while LiZrPtTl reaches W···at − 0.072 eV at 1200 K. The PF peaks at 1200 K for both alloys and decreases at lower temperatures. These high PF values near the Fermi level suggest that even small doping can significantly enhance thermoelectric performance. Finally, the thermoelectric figure of merit (ZT) as a function of chemical potential is shown in Fig. 9(e, f). At room temperature, ZT for both alloys reaches ≈ 0.96 near the Fermi level. Within the chemical potential range of 0.32–0.53 eV, ZT stabilizes at ≈ 0.99, indicating excellent thermoelectric performance. The behavior of ZT with temperature and chemical potential shows a clear distinction between p-type and n-type regions: in the p-type regime, ZT increases with temperature due to enhanced carrier mobility and reduced lattice thermal conductivity contributions, while in the n-type regime (0–0.62 eV), ZT decreases with temperature. This comprehensive analysis demonstrates that careful tuning of chemical potential (i.e., controlled doping) can optimize both the Seebeck coefficient and power factor, thereby maximizing the thermoelectric efficiency of LiMPtTl alloys for high-temperature energy conversion applications88,89. Figures 9(g, h) illustrate the dependence of electrical conductivity ((/() on chemical potential. In both alloys, (/( is found to be negligible within the chemical potential range of 0.25–0.85 eV, which is in accordance with the existence of the band gap, and a substantial rise is observed outside this range. However, a contrary behavior is noticed beyond − 0.75 eV. The maxima of are found to be on the negative side of the chemical potential, which is an indication of p-type semiconducting properties, where holes are the charge carriers. The electronic thermal conductivity () is presented in Fig. 9(i, j). Within the chemical potential range of 0.08–0.75 eV, is nearly zero, consistent with the insulating behavior near the band gap. As temperature increases from 300 K to 1200 K, rises substantially for both alloys, indicating enhanced thermal transport by charge carriers at elevated temperatures. This trend also correlates with the increase in electrical conductivity and highlights the close relationship between electronic heat transport and carrier mobility. Thermodynamic properties Lattice-vibration-related thermodynamic behavior plays an important role in the assessment of material applicability to electronic and energetic devices90,91. Temperature-dependent quasi-harmonic Debye approximation methods were applied by employing the GIBBS292, program to understand the thermodynamic response of LiTiPtTl and LiZrPtTl alloys. Therefore, the key quantities to be determined included Cv (heat capacity at constant volume), Grüneisen parameter, entropy, Debye temperature, thermal expansion coefficient, and Helmholtz free energy as a function of temperature for LiMPtTl (M = Ti, Zr) alloys and are plotted in Fig. 10. (a) Heat capacity at constant volume Cv, (b) Entropy S, and (c) Free energy, (d) Debye temperature θD for QH alloys QHH LiMPtTl (M = Ti, Zr). As shown in Fig. 10(a), Cv increases steeply below 300 K according to the Debye T³ dependence and increases gradually to a limiting value at higher temperatures. The saturation values of approximately 94.79 J mol⁻¹ K⁻¹ for LiTiPtTl and 94.89 J mol⁻¹ K⁻¹ for LiZrPtTl are in agreement with the classical Dulong–Petit limit93,94. The identical behavior exhibited by both alloys reflects stable lattice vibrations and thermodynamic reliability in a wide temperature interval, supporting their suitability for thermal applications. Figure 10(b) depicts the influence of temperature on Helmholtz free energy. It is clear that with an increase in temperature, there is a constant decrease in free energy, as depicted by A=E-TS. From 0 K, it changes from 11.79 J mol⁻¹ K⁻¹, 11.52 J mol⁻¹ K⁻¹, to -223.48 J mol⁻¹ K⁻¹, -216.08 J mol⁻¹ K⁻¹, respectively, for LiTiPtTl, LiZrPtTl. From the calculated entropy value and Fig. 10(c), we notice that entropy increases as the temperature increases for the two compounds. This corresponds to the expected phenomenon where entropy increases as the temperature increases and lattice vibrational motion occurs. When the entropy value is inspected at a specific temperature of 300 K, we note that the entropy value is 133.82 J mol⁻¹ K⁻¹ for LiTiPtTl and 134.81 J mol⁻¹ K⁻¹ for LiZrPtTl. In comparison, the LiTiPtTl system has a higher value of entropy, which may be attributed to lattice vibrational motion. The Debye Temperature93 helps in understanding the stiffness and vibrational characteristics of the lattice. For the alloys LiTiPtTl and LiZrPtTl, when going to absolute zero using the above-mentioned formula to calculate they are found to be 315.3 K and 308.09 K, respectively. This shows that the lattice is stiffer in the case of LiTiPtTl. This is in agreement with the trends of lattice thermal conductivity as shown in Fig. 10(d). Moreover, these results indicate that the alloys exhibit very stable thermal characteristics and can be used for high-temperature thermoelectric devices. The lattice anharmonicity is measured by the Grüneisen parameter ((), which is dependent on how the vibrational frequencies change with volume. Lattice thermal conductivity, thermal expansion, and phonon scattering can all be better understood with the help of the Grüneisen parameter. The Grüneisen parameter values for LiMPtTl (M = Ti, Zr) alloys at absolute zero temperature and pressure are 2.70 for LiTiPtTl and 2.20 for LiZrPtTl. As shown in Fig. 10(e), the slightly higher in LiZrPtTl indicates enhanced lattice anharmonicity, leading to stronger phonon-phonon interactions and increased scattering, which contributes to reduced lattice thermal conductivity at high temperatures94–96. These results underscore the influence of on the thermal and thermoelectric behavior of these quaternary Heusler alloys. It is also closely related to anharmonicity and phonon scattering. Herein, ( of LiTiPtTl and LiZrPtTl is estimated to be 5.85 × 10⁻⁶ K⁻¹ and 4.28 × 10⁻⁶ K⁻¹ at room temperature, respectively. From Fig. 10f, one can find that LiZrPtTl has a slightly higher thermal expansion compared with LiTiPtTl, reflecting its enhanced lattice anharmonicity. These values further support the above-mentioned trends observed in lattice thermal conductivity and consequently confirm that both alloys possess good thermal stability for high-temperature thermoelectric application. Conclusion The structural stability, band structure, thermodynamic properties, elastic properties, and optical properties of the QH LiMPtTl (M = Ti, Zr) compounds were investigated using density functional theory calculations based on the FP-LAPW method. The volume optimization calculations show that the two alloys are stable in the type-3 arrangement of the face-centered cubic (FCC) structure, as suggested by their calculated formation energies. The band structure calculations show that the two compounds are indirect band gap semiconductors. The band gap energy of LiTiPtTl is found to be 0.84 eV. In the case of LiZrPtTl, the value of the band gap is 0.99 eV. In both cases, the band gap is due to the contribution of the 3d/4d orbitals of the Ti/Zr atom and the 5d orbital of the Pt atom. Phonon dispersion curves provide clear evidence of the dynamical stability of the compounds. From the Dulong-Pettit theorem and the Debye model of solids at high and low temperatures, respectively, it can be said that the compounds are thermodynamically stable. Calculations of elastic properties indicate that both alloys are mechanically stable, brittle, and anisotropic. Optical properties, such as high dielectric constants, large optical conductivity in the visible range, and high absorption. High UV reflectivity also indicates the possibility of using these alloys in solar shielding coatings. Moreover, the thermoelectric properties have been calculated using the semiclassical Boltzmann transport equations. The calculated values of ZT are found to be 0.73 and 0.70 for LiMPtTl (M = Ti, Zr) alloys, respectively, which are relatively higher and more stable than other QH alloys, indicating that these alloys are promising materials for thermoelectric, optoelectronic, and photovoltaic devices. Future experimental work is required to confirm these theoretical predictions. Supplementary Information Below is the link to the electronic supplementary material. Supplementary Material 1 Acknowledgments Princess Nourah bint Abdulrahman University Researchers Supporting Project number (PNURSP2026R55), Princess Nourah bint Abdulrahman University, Riyadh, Saudi Arabia. Author contributions All persons who meet authorship criteria are listed as authors, and all authors certify that they have participated sufficiently in the work to take public responsibility for the content, including participation in the concept, design, analysis, writing, or revision of the manuscript.Ramesh Sharma, Ali B. M. Ali, Jisha Annie Abraham, Jaya Madan- Conceptualization, Methodology, Investigation, formal analysis, Software, Writing- Original draft preparation, Supervision.Nikhil Shrivastav, Sabirov Sardor, Mirjalol Ismoilov, F. F. Al-Harbi, Awatif Alshamari– Writing Original draft preparation, Visualization, Investigation. Writing- Reviewing and Editing, funding acquisition. Data availability The datasets used and/or analysed during the current study available from the corresponding author on reasonable request. Declarations Competing interests The authors declare no competing interests. Footnotes Publisher’s note Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations. References Associated Data Supplementary Materials Supplementary Material 1 Data Availability Statement The datasets used and/or analysed during the current study available from the corresponding author on reasonable request.