A detailed investigation of a-IGZO thin film-based MSM UV photodetector Authors: Tarik Asar Published: 2026 ABSTRACT AbstractAmorphous Indium–Gallium–Zinc–Oxide (a-IGZO) thin films were deposited on silicon and glass substrates using a magnetron sputtering system at room temperature. The structural, morphological, optical, and electrical properties of the films were systematically investigated to evaluate their suitability for ultraviolet photodetection. Secondary Ion Mass Spectrometry and Atomic Force Microscopy were employed to characterize the film composition and surface topology, while Hall Effect and Current–Voltage measurements were used to assess the electrical performance. The optical properties were analyzed in the 200–1100 nm spectral range using UV–VIS spectroscopy. A Metal–Semiconductor–Metal (MSM) photodetector was fabricated using a-IGZO film. The average transmittance of the film is 80%, an estimated optical energy gap value is 3.1 eV, and the band tail width is 382 meV. The electrical results for carrier density, mobility, and resistivity were determined to be 4.88 × 1019 cm− 3, 7.83 cm2/V.s, and 1.64 × 10− 2 Ω.cm, respectively. The FoM is calculated as 1.27 × 10− 4 Ω−1. a-IGZO MSM photodetector output parameters at 385 nm ultraviolet illumination, such as responsivity, detectivity, noise equivalent power, photo-to-dark current ratio, and normalized photo-to-dark current ratio at the critical voltage are determined as 12.72 A/W, 1.13 × 1013 Jones, 7.69 × 10− 13 W/Hz1/2, 0.386, and 3.96 × 105 W− 1, respectively. The results demonstrate that the a-IGZO MSM device exhibits behaviors comparable to those in the literature of ultraviolet photodetectors, confirming the potential of a-IGZO as a promising material for advanced optoelectronic applications.Supplementary InformationThe online version contains supplementary material available at 10.1038/s41598-026-52983-w.Keywords: Indium–Gallium–Zinc–Oxide, Metal–Semiconductor–Metal, UV photodetector, Thin film characterization, Device characterizationSubject terms: Materials science, Nanoscience and technology, Optics and photonics, Physics Introductıon Transparent conducting oxide (TCO) is essential for variety of optoelectronic applications devices1,2, such as at-panel displays3, touch screens4, gas sensors5, organic light emitting diodes6, electrochromic devices7, transistor8, lenses9, transparent electrodes in LCD screens10, and photodetectors (PDs)11. Among TCOs, Amorphous Transparent Oxide Semiconductors (ATOSs) have attracted considerable attention due to several promising features, including high transparency in the visible light region, high free-carrier mobility, and large-area, uniform deposition even at room temperature12–17. ATOSs are generally classified into two groups: single cation systems, such as Zinc-Oxide (ZnO)18, Tin-Oxide (SnO)19, and multi-cation systems that include Zinc-Indium-Oxide (ZnInO)20, Zinc-Tin-Oxide (ZnSnO)18, Gallium Zinc Oxide (GaZnO)21, and Indium-Gallium-Zinc-Oxide (InGaZnO)16,18,22. Because mixing two or more cations with different ionic sizes and charges greatly promotes the formation of the amorphous phase, using a multi-cation system helps ensure that thin films remain amorphous during processing18,23. Amorphous-InGaZnO (a-IGZO) is one of the most promising semiconductor oxide materials because of its high electron mobility, low leakage current, good film uniformity, optical transparency, and compatibility with low-temperature, large-area fabrication24–26. Additionally, a variety of optoelectronic applications, including transparent electronics, neuromorphic vision, sensors, and UV PDs, have been enabled by IGZO’s ultraviolet (UV) light absorption properties, owing to its broad optical band gap (Eg) of approximately 3.3–3.5 eV27–29. Among various deposition techniques for a-IGZO thin films, RF sputtering, which has the advantages of good film adhesion, reproducibility, high deposition rate, good homogeneity, and suitability for large-area processing, is one of the most widely used in many industries to prepare transparent and conductive thin films30–34. The sputtering method allows for the accurate transfer of target material stoichiometry to the deposited film35. By modulating parameters such as the sputtering power and the oxygen partial pressure during deposition, researchers can precisely control the concentration of oxygen vacancies, which are the primary source of free carriers in IGZO36–38. Lowering the carrier concentration through controlled oxidation is essential to ensure that the Schottky contact depletion region extends sufficiently across the channel to suppress dark current36–39. Furthermore, the high kinetic energy of atoms arriving at the substrate during sputtering (typically 1–10 eV) promotes adatom migration, resulting in dense, compact, and smooth amorphous structures36–40. Unlike solution-processed methods, sputtering produces films with low surface roughness and fewer structural defects, which is crucial for forming reliable, reproducible Schottky interfaces in Metal-Semiconductor-Metal (MSM) devices37–40. A significant advantage of magnetron sputtering is also its ability to deposit high-quality films at room temperature or low processing temperatures17,35–40. Thus, the magnetron sputtering systems provide the necessary control over material density, carrier concentration, and interface morphology to realize high-performance, stable, and scalable a-IGZO-based MSM photodetectors for next-generation UV sensing technologies. These properties make a-IGZO suitable for a variety of applications, including PDs41–44. PDs are well-suited optoelectronic devices for monitoring the exposure limit to UV radiation. Their extensive use has enabled various applications, including space communications, medical applications, flame detection and surveillance, missile tracking, environmental condition assessment, and UV emission identification45,46. These advantages make it highly promising for a wide range of applications in both military and civilian fields48. Therefore, it is important to develop an effective sensor for UV light detection28. UV PDs are crucial in advancing science and technology by transforming optical signals into electrical signals using semiconductor materials45. One notable application of a-IGZO is in MSM photodetectors. The MSM photodetector architecture, characterized by its fast photoresponse, benefits substantially from the integration of IGZO, enabling its use in advanced optoelectronic systems that require both high performance and stability44,47. The basic structure of an MSM photodetector typically consists of a semiconductor layer sandwiched between two metal electrodes, often configured as interdigitated fingers to optimize carrier collection48–50. This interdigitated design enhances the electric field in the semiconductor, facilitating the efficient separation and collection of photogenerated electron-hole pairs and thereby improving responsivity and speed49. For IGZO MSM photodetectors, a-IGZO films are often used due to their uniform properties and suitability for low-temperature processing, including room-temperature fabrication47. The judicious selection of metal contacts is crucial, as the metal-semiconductor interface properties, particularly the Schottky barrier height, significantly influence device performance, including dark current and photoresponse51,52. For instance, asymmetric electrode designs using different metals can yield varying Schottky barrier heights, enabling self-powered photodetection even without an applied bias53. Self-powered photodetection devices offer several advantages, including low power consumption, reduced system complexity, compact size, and simplified fabrication. Those devices can be divided into two groups according to the method of energy conversion: one type includes photoconductive devices, which convert UV radiation into electrical energy; the other type includes photovoltaic (built-in electric field) devices containing p–n junctions, heterojunctions, or Schottky junctions54–60. In photovoltaic mode, which means the incoming light signal induces spontaneous diffusion of free-carriers through the space charge region and electron-hole separation that leads to current flow at zero-bias voltage61. Usually, a built-in electric field, which separates the photogenerated electron-hole pairs and gives rise to a circuit current, is formed due to the spontaneous diffusion of electrons driven by the work function difference between the contact metal and the semiconductor. Unfortunately, the semiconductor’s surface state can significantly affect the diffusion process. The photoresponse at zero bias can also occur from a nonuniform distribution of trap densities at the metal/semiconductor interface. If the barrier heights at the surface states can be modulated, an asymmetric Schottky barrier forms, providing an additional driving force for the spontaneous diffusion of photocurrent in MSM PDs62. Asymmetric contacts receive significant recognition for enhancing the self-assembly of the built-in field to separate electron-hole pairs without an external bias, with significant Schottky contact differences, and supporting the long-term operation of the device63. Additionally, the photoresponse at zero bias can be attributed to hole trapping. The hole-trapping process at the metal electrode/a-IGZO interface plays an important role in achieving unbiased photoresponse in a-IGZO UV PDs. It provides insight into the operation of an a-IGZO UV PD at zero bias using a simple MSM structure47. Furthermore, the spectral response of IGZO MSM photodetectors can be tuned, for example, to enhance sensitivity in the solar-blind UV window by optimizing the deposition environment64. In terms of specific performance metrics, IGZO MSM photodetectors have achieved notable results. A maximum responsivity of 120 A/W and a noise equivalent power of 0.2 nW/(Hz)1/2 with a response time of 30 ms have been reported for real-time UV photodetectors fabricated with a-IGZO and gold electrodes44. This performance highlights the potential of a-IGZO in UV sensing and related optical applications. Therefore, the development of IGZO MSM photodetectors expands the range of photodetector technologies, which are essential in fields such as imaging, self-powered systems, remote communications, security, and wearable electronics65. Ongoing research into materials such as IGZO, along with advancements in device architecture and integration, promises further improvements in the performance and versatility of these devices. The characterization of a-IGZO thin films and IGZO MSM UV photodetectors, including their structural, morphological, optical, and electrical properties, has significant implications. In this study, a-IGZO thin films were deposited at room temperature on both silicon and glass substrates using magnetron sputtering. The structural, morphological, and optical characterizations of the deposited a-IGZO thin film and electrical behaviors of the IGZO MSM UV Photodetector were determined by Secondary Ion Mass Spectrometer, Atomic Force Microscope, Hall Effect, and Current-Voltage measurement systems. The optical characterization of the a-IGZO thin film was determined in the spectral region of 200–1100 nm by a UV-Vis spectrometer. The electrical output parameters of the fabricated IGZO MSM UV Photodetector, such as Responsivity (R), Detectivity (D*), Noise Equivalent Power (NEP), Photo-to-Dark Current Ratio (PDCR), and Normalized Photo-to-Dark Ratio (NPDR), were determined to assess the effect of electrical parameters on device performance. Experimental a-IGZO thin films were deposited on both the n-type Si substrate (Si stands out as a more cost-effective option and owing some advantages32, having a resistivity range of 1–10 Ωcm, and the Corning glass substrate by means of the RF magnetron sputtering system (Nanovak NVTS-500), having an InGaZnO4 target (Kurt J. Lesker, 99.99% Pure, 2.00” Diameter x 0.125” Thick). Before the deposition process, n-type Si and Corning glass substrates were cleaned with an inorganic solvent of CH3COCH3 in an ultrasonic bath for 10 minutes, followed by a second cleaning with an inorganic solvent of CH3CH(OH)CH3. After rinsing with deionized (DI) water, the n-type Si substrate was finally dried with N2 and then loaded into the magnetron sputtering system. After that, the a-IGZO thin films were deposited on the front surfaces of both substrates without oxygen. The deposition parameters are given in Table 1. Table 1RF sputtering deposition parameters of a-IGZO thin film.ParametersValuesChamber Base Pressure3 × 10− 6 torrChamber Deposition Pressure5 × 10− 3 torrAr Flow3.8 sccmO2 Flow0 sccmAr: O2100:0RF Power Set 1 (Target Heating Power/Before Shutter Opening)70 WRF Power Set 1 Ramp0.2 W/sRF Power Set 1 Time300 sStanding Time on Set 1 Power300 sRF Power Set 2 (Deposition Power)100 WRF Power Set 2 Ramp0.5 W/sRF Power Set 2 Time60 sDeposition TemperatureRoom Temp.Rotation of The Sample5 rpmDeposition Rate1.3 Å/sDeposition Time770 sEstimated Deposition Thickness (from QCM)100 nmThin Film Thickness (from profilometer)95 nm RF sputtering deposition parameters of a-IGZO thin film. Then, an IGZO MSM UV photodetector was fabricated on 10 × 10 mm2 Si-based sample. The fabrication process included a native oxide removal step and an MSM diode-forming step that involves two back-to-back Schottky interdigital electrodes. First, the native oxide on the Si substrate surfaces was removed using a wet-chemical etch solution of 1H2SO4:1H2O2:80 DI-H2O for 1 minute. The samples were rinsed in DI-H2O and dried with nitrogen gas. After that, Ag interdigital electrodes with a 100 μm line width, 100 μm spacing, and 800 μm length were deposited onto an a-IGZO thin film-coated n-Si substrate using the Aerosol Jet Printing System (Aerosol Jet 5X Systems; Optomec, USA). A schematic representation of the fabricated IGZO MSM UV photodetector device is given in Fig. 1. Schematic presentation of IGZO MSM UV photodetector device. The structural, morphological, and optical characterizations of the deposited a-IGZO thin films and electrical behaviors of the IGZO MSM UV Photodetector were determined by Secondary Ion Mass Spectrometer (Hiden SIMS Workstation), Atomic Force Microscope (Nanomagnetics Instruments), Hall Effect (Lake Shore HMS), and Current-Voltage (Keithley 4200-SCS) measurement systems. The optical characterization of the a-IGZO thin film was determined in the spectral region of 200–1100 nm by an UltraViolet-Visible (UV-Vis) spectrometer (PerkinElmer Lambda 2 S). The electrical output parameters of the fabricated photodetector, including Responsivity (R), Detectivity (D*), Noise Equivalent Power (NEP), and Normalized Photo-to-Dark Ratio (NPDR), were determined by analyzing the results obtained from Current-Voltage measurements performed under ultraviolet light at room temperature. Results and dıscussıons a-IGZO thin film characterization The deposited IGZO thin film was confirmed to be amorphous in our previous study using Grazing Incidence X-Ray Diffraction (GIXRD), in which the X-Ray beam incidence angle was kept at a very low angle to focus solely on the thin-film surfaces66. It is also well known that surface morphology is a crucial factor in determining the performance of electro-optical devices, such as MSM photodetectors, solar cells, LEDs, and sensors67. In devices such as MSM photodetectors, which will be produced on a rough, thin-film surface, distortions at the metal-semiconductor interface may occur, potentially affecting device performance. For this reason, it is essential to examine thin-film surfaces using surface analysis methods, such as AFM, to achieve successful surface functionalization and to determine the Root Mean Square (RMS) roughness values using suitable software68. Thus, the surface morphology of the structure over a 3 μm × 3 μm area was characterized using the obtained AFM measurements. Figure 2 shows the two-dimensional (2D) and three-dimensional (3D) AFM images of the a-IGZO thin film surface, illustrating its morphology and surface roughness. The sample’s surface RMS roughness is 0.90 nm. However, the a-IGZO thin film surface has poles with heights of 6.35 nm distributed across the film surface. The formation of these poles could be due to the rapid sublimation of starting materials before decomposition69. (a) 2D and (b) 3D AFM images of a-IGZO thin film. The surface appears smooth, which enhances the device’s high electrical performance70,71, as surface defects are primary candidates for causing cracks in the film under external stresses71. The smooth, thin film surface played a crucial role in high-performance devices72. The surface construction is nearly identical to that in the literature for oxide-based thin films17,73. The interface characteristics of an a-IGZO thin film were analyzed using Secondary Ion Mass Spectroscopy (SIMS) depth profile measurements. SIMS is a destructive technique used to analyze a material’s composition. This method involves removing material by sputtering and then analyzing the ejected particles with a mass analyzer67,74. SIMS depth profile of the In, Ga, Zn, O2, and Si atoms in the sample is given in Fig. 3. SIMS depth profile of a-IGZO thin film. In the SIMS graph, it is evident that there is a sharp transition between the atoms forming the a-IGZO thin film and the n-Si substrate. This transition between the atoms and the substrate also indicates that the a-IGZO thin film is approximately 95 nm thick. Additionally, it is worth noting that O2 diffusion into the substrate layer is negligible at the end of thin film deposition. At the interface between the a-IGZO thin film layer and the substrate, the number of materials forming the thin film decreases. In contrast, the amount of Si as the substrate material increases significantly. This good interfacial formation also demonstrates that the thin film forms on the substrate with high quality and surface compatibility. This situation is encountered in many thin films produced from high-quality semiconductor substrates in literature. The transmittance (T) and reflectance (R) characteristics of thin films can reveal their optical properties, which depend strongly on the film thickness, microstructure, impurity levels, and deposition parameters75. For that, the normal-incidence transmission spectra of a Corning glass substrate with and without a thin film were measured by UV-VIS spectrophotometry in the 200–1100 nm wavelength range. Figure 4 shows the optical transmission for the a-IGZO thin film. It was found that the film’s average transmittance is 80%. Additionally, the inset of Fig. 4 shows the reflectance behavior of the thin film. The transmittance and reflectance behavior of the a-IGZO thin film dependent on wavelength. The additional optical behavior of a-IGZO thin film has also been examined to investigate the nature of the optical transitions, which involve absorption coefficient, band gap, and Urbach energy at room temperature76. Suppose the film thickness (d) is known. In that case, the wavelength-dependent transmittance and reflectance spectra derived from the obtained UV-Vis data can be used to determine the optical absorption coefficient (α). For that aim, the following equations can be accessed77,78: Figure 5 shows the wavelength dependence of the optical absorption coefficient spectra of the a-IGZO thin film. That spectrum evinces that the absorption edge is nearly observed at the beginning of the visible region. It can be said that the position of the absorption edge depends on the composition of the thin film76. The wavelength-dependent optical absorption coefficient spectra of a-IGZO thin film. Furthermore, it can also be stated that the optical density (OD) varies in proportion to the thickness of the a-IGZO thin film, with a relationship between them as OD = αd78. In general, α can be related to hυ by the known equation, as Tauc’s relations30,31,66,79–81. Where ξ, Eg and n are the constants describing the band tailing parameter, the band gap energy, and the power factor of the transition mode, respectively. n is also essential and is dependent upon the crystalline nature of the material (crystalline or amorphous). Amorphous materials, including a-IGZO thin films, have an indirect transition82,83 In this case, it would be appropriate to take n = 2, hence: Therefore, the plotting of (αhυ)1/2 - (hυ) yields a straight line in a particular region. As seen in Fig. 6, the extrapolation of this straight line will intercept the (hυ)-axis to give the value of the indirect optical energy gap (Eg) of a-IGZO thin film84. Thus, an estimated value for the a-IGZO thin film is 3.1 eV, which is compatible with the literature28,85,86. The (αhυ)1/2- (hυ) graph of a-IGZO thin film that gives the indirect optical energy gap (Eg). Generally, low optical absorption can result from a higher band gap value. Low visible-range absorption is observed in most metal oxide semiconductors, which have band gaps above 3 eV85. Additionally, Eq. (5) can be rearranged to verify whether the optical bandgap transition in an IGZO thin film is direct or indirect, as follows87: Hereby, the plotting of ln(αhυ) on y-axis against ln(hυ)-Eg on the x-axis, as Fig. 7 shows, a straight line is given, and the slope determines the power factor (n)84,87. The determined n value of the a-IGZO thin film is 2.02, which is proof that it is used correctly in Eq. (6). The ln(αhυ)-ln(hυ)-Eg) graph. Furthermore, Urbach energy (EU), also known as band-tail energy, is another critical parameter of most non-crystalline semiconducting materials, such as a-IGZO, and can be determined from UV-Vis spectra88. Urbach energy can also be identified as the band-tail width of the localized states within the optical energy gap. The relationship between the absorption coefficient (α) and photon energy (hυ), known as the Urbach empirical rule, is described by an exponential equation and becomes particularly important near the optical band edge. Where α0 is a constant. The ln(α)-(hυ) behavior of a-IGZO thin film near the absorption edge is shown in Fig. 8. Dependence of ln(α) upon hυ for a-IGZO thin film. The Urbach energy is calculated by obtaining a straight line on the ln(α)-hυ graph. The reciprocal of the slope in the linear region below the optical band gap yields the value of EU89. The obtained band-tail width is 382 meV. Lower crystallinity and disorder in semiconductor materials can originate from higher Urbach energy88. IGZO MSM UV photodetector characterization When the IGZO thin film is under UV illumination (typically with photon energy greater than the IGZO bandgap), several processes occur simultaneously, including photogeneration, oxygen desorption, and ionization of oxygen vacancies27,28. UV photons excite electrons from the valence band to the conduction band, generating electron-hole pairs28,46. The electron–hole pairs are generated, and the photogenerated holes are captured by adsorbed oxygen ions. Then, these oxygen ions become oxygen molecules again and desorb from the IGZO thin film ()21. This process “releases” the previously trapped electrons back into the conduction band27. UV light also ionizes oxygen vacancies (), promoting electrons to the conduction band ()27,46. The trapping of photogenerated holes by surface oxygen ions delays carrier recombination. Because holes are consumed at the surface via desorption, the lifetime of photogenerated electrons is extended, allowing them to circulate through the circuit multiple times21. This results in photoconductive gain and transition efficiency21,28. A model using an energy band diagram to explain the working principle of a self-powered PD at zero bias is shown in Fig. 9. The energy band diagrams for a self-powered IGZO MSM photodetector at 0 V in the dark and under ultraviolet illumination62. The electrical characteristics of the a-IGZO thin film, including resistivity, carrier density, and mobility, were determined using the Van der Pauw method, and the data were obtained from a Hall Effect System. The obtained resistivity, carrier density, and mobility values are shown in Table 2, along with literature values. Table 2Comparison of the hall effect measurements obtained results with the literature. Resistivity (Ω.cm) Carrier Density (cm−3) Mobility (cm2/V.s) Reference 1.64 × 10−2 4.88 × 1019 7.83 [Present study] 2.40 × 10− 1 3.41 × 1018 7.71 90 8.85 × 10−3 4.98 × 1019 5.83 91 1.04 × 10−2 5.50 × 1019 10.98 92 1.20 × 10−2 1.60 × 1019 ~ 35.00 93 Comparison of the hall effect measurements obtained results with the literature. The examined thin film was found to be of the n-type. The oxygen vacancies in a-IGZO thin films can act as shallow donors that effectively supply conduction electrons, also simultaneously acting as scattering centers that effectively reduce charge carrier conduction to a certain extent. The impact of scattering centers is observed to be greater in this study, as indicated by the literature90–93. The Figure of Merit (FoM, ΦH) is a critical parameter for transparent oxide semiconductors. A higher FoM value indicates better-quality TCO films94,95. The FoM was computed using the following equation, suggested by Haacke96: Where Rs represents the sheet resistance and T denotes the transmittance. In this method, the FoM is determined using the sheet resistance and the optical transmission of the transparent conductor at the wavelength near the maximum of the solar spectrum (≈ 550 nm)97,98. The FoM is calculated as 1.27 × 10− 4 Ω−1, which is close to the published reference works, as shown in Table 394,99–101. Table 3Comparison of the obtained FoM value with the literature. Film Type Figure of Merit (Ω−1) Reference a-IGZO 1.27 × 10−4 [Present study] IGZO 2.00 × 10−5 94 IGZO 6.85 × 10−5 99 IGZO/TiO2 1.44 × 10−4 99 IGZO/Cu 2.60 × 10−4 94 IGZO/Cu/IGZO 6.00 × 10−3 100 IGZO/Ag/IGZO 45.02 × 10−3 101 Comparison of the obtained FoM value with the literature. The voltage-dependent current behavior of a-IGZO MSM photodetector with and without UV light exposure (385 nm) is seen in Fig. 10. Without light exposure, the measured currents are below 345 µA. For each detector, the minimum current is recorded at an applied voltage of 0 V44. The light exposure results in an increase of 6375 µA in the current. The current-voltage behavior of a-IGZO MSM UV photodetector. In general, the current increases with increasing voltage, both in the presence and absence of light. Theoretically, the detectors are designed symmetrically, which should lead to symmetrical I-V curves. Slight deviations may be caused by fabricating imperfections, which lead to different Schottky barrier strengths at the two electrode semiconductor interfaces. Additionally, the figure-of-merit characterizing the photodetector’s performance includes Responsivity (R), Detectivity (D*), Noise Equivalent Power (NEP), Photo-to-Dark Current Ratio (PDCR), and Normalized Photo-to-Dark Current Ratio (NPDR)102. A light source with a wavelength of 385 nm is used to examine the devices’ optical response properties. As we all know, R is a key factor in determining a photodetector’s light-sensitivity103,104. Responsivity is the conversion efficiency from optical input to electrical output. Responsivity depends on the wavelength, the light power, the voltage between the electrodes, and the temperature. It also describes how strongly the current depends on the light power on the photodetector. Responsivity in A/W is defined as follows: Where Iphoto refers to the current difference between the dark condition and the illuminated condition, Pλ represents the total power used to illuminate the device, Idark is the current measured in the dark, and Ilight is the current measured when the device is subjected to the illumination source44,56,104,105. Figure 11 shows the voltage-dependent responsivity behavior of the a-IGZO MSM photodetector. As the voltage increases, the responsivity rises to nearly 3 V before decreasing. The same behavior has been observed previously in photodetectors106–108. The responsivity behavior of the a-IGZO MSM UV photodetector. It is expected that at a critical voltage, the semiconductor will be damaged due to heating caused by the high current flow44. For that device, the critical voltage is 3.02 V. The highest measured responsivity, 48.99 A/W, was taken at room temperature at the critical voltage. The produced photodetector exhibits higher sensitivity than both commercially available silicon-based photodiodes and research-and-development photodiodes, such as ZnO, Si PIN, and InGaAs109–112. Additionally, determining the specific detectivity (D*) is a key aspect of photodetector evaluation. This highlights the crucial role of dark current measurements, as detectivity is highly dependent on them. A high dark current can introduce significant noise, negatively impacting the detector’s performance. Thus, reducing the dark current as much as possible is crucial for enhancing the detection limit and reducing power consumption113. It is also known that the specific detectivity of a photodetector represents the ability to detect weak optical signals, which can be calculated via the equation below: In this expression, R refers to responsivity, A represents the active area of the photodetector, e represents the elementary charge, and Idark corresponds to the dark current measured in the device102,105,114. The fabricated a-IGZO MSM photodetector shown in Fig. 12 reaches a detectivity of 4.37 × 1013 Jones at an applied bias of 0.79 V. As depicted in the figure, the calculated detectivity at voltages below 1 V is significantly higher than that of IGZO/Cr-PE, pristine IGZO, and p-GaN/n-IGZO photodetectors64,115. The specific detectivity behavior of the a-IGZO MSM UV photodetector. Additionally, NEP is a standard metric that quantifies a photodetector’s sensitivity116. NEP is defined as the incident radiant power that generates a signal voltage equal to the detector’s noise voltage. It corresponds to the minimum optical excitation required to produce a signal with a 1 Hz noise bandwidth. The NEP can also be calculated using one of the following two formulas102,117: Where D* is specific detectivity, A is the effective photodetector area in cm2, and Δf is the electrical bandwidth in Hz. NEP for evaluating the noise characteristic of an a-IGZO MSM photodetector is shown in Fig. 13. Because the NEP is tightly linked to responsivity, it reaches its lowest values at approximately 0.5 V to 3.5 V. In detail, the lowest NEP is observed at 0.79 V, corresponding to 2.29 × 10− 13 W/Hz1/2. The noise equivalent power behavior of the a-IGZO MSM UV photodetector. An additional important performance metric of the photodetector, the PDCR (photo-to-dark current ratio), and the NPDR (normalized photo-to-dark current ratio) were further studied. PDCR and NPDR are also significantly influenced by dark current-like detectivity. PDCR can be expressed as the following118,119: NPDR can be expressed as the following115,120: Where Iphoto is the difference current of the dark field to light field, Pλ is the total power at which the device is illuminated, Idark is the dark field effect current, Ilight is the field effect current when exposed to an illumination source, and A is the effective photodetector area in cm2. The voltage-dependent PDCR and NPDR characteristics of the a-IGZO MSM photodetector are shown in Fig. 14. In detail, the highest PDCR and NPDR are observed at 0.14 V, corresponding to 31.207 and 9.202 × 106 W− 1, respectively. The PDCR and NPDR characteristics of the a-IGZO MSM UV photodetector. The a-IGZO UV Photodetector performance results, as Responsivity (R), Detectivity (D*), Noise Equivalent Power (NEP), Photo-to-Dark Current Ratio (PDCR), and Normalized Photo-to-Dark Current Ratio (NPDR) at the critical voltage, minimum value points, and maximum value points are given in Table 4. Table 4a-IGZO UV photodetector output parameters.Photodetector Output ParametersValues @ VoltageMinimum Current at Dark 345 µA @ 0 V Minimum Current Under Illumination 6375 µA @ 0 V The Critical Voltage 3.02 V Maximum R 48.99 A/W @ 3.02 V R at The Critical Voltage 48.99 A/W @ 3.02 V Self-Powered R 0.172 A/W @ 0 V Maximum D*4.37 × 1013 Jones @ 0.79 VD* at The Critical Voltage1.13 × 1013 Jones @ 3.02 VSelf-Powered D*0.50 × 1013 Jones @ 0 VMinimum NEP2.29 × 10− 13 W/Hz1/2 @ 0.79 VNEP at The Critical Voltage7.69 × 10− 13 W/Hz1/2 @ 3.02 VSelf-Powered NEP0.198 × 10− 13 W/Hz1/2 @ 0 VMaximum PDCR 31.207 @ 0.14 V PDCR at The Critical Voltage 0.386 @ 3.02 V Self-Powered PDCR 17.44 @ 0 V Maximum NPDR9.202 × 106 W− 1 @ 0.14 VNPDR at The Critical Voltage3.96 × 105 W− 1 @ 3.02 VSelf-Powered NPDR5.08 × 105 W− 1 @ 0 V a-IGZO UV photodetector output parameters. As shown in Table 5, the obtained photodetector parameters, such as responsivity and detectivity at the UV wavelength and at zero bias, are consistent with the literature. Furthermore, to the best of our knowledge, we have not encountered any other comprehensive study like this one that presents the output parameters of an IGZO MSM UV photodetector at zero bias, including responsivity, detectivity, noise equivalent power, photo-to-dark current ratio, and normalized photo-to-dark current ratio. Table 5Comparison of the photodetector output parameters at zero bias with the reported self-powered ultraviolet photodetectors.Material/StructureWavelength (nm)R (A/W)@ 0 VD* (Jones)@ 0 VReferences a-IGZO/n-Si MSM 385 172 × 10−3 0.50 × 1013 [Present study] p-GaN/IGZO 340 260 × 10−3 1.9 × 1013 115 NiO/a-IGZO 365 29 × 10−3 699 × 1013 121 a-IGZO/p-Si 325 8 × 10−3 117 × 1013 122 p-GaN/IGZO 350 960 × 10−3 3.46 × 1013 123 MoS2 /a-InGaZnO/a-Ga2O 3 254 183 × 10−3 1.52 × 1013 124 Comparison of the photodetector output parameters at zero bias with the reported self-powered ultraviolet photodetectors. Conclusıons The amorphous Indium–Gallium–Zinc–Oxide (a-IGZO) thin films were deposited at room temperature. The structural, morphological, optical, and electrical properties of the films were systematically investigated to evaluate their suitability for ultraviolet photodetection. It was found that the average transmittance of the film is 80%, an estimated optical energy gap value is 3.1 eV, and the band tail width is 382 meV. The electrical results for carrier density, mobility, and resistivity were determined to be 4.88 × 1019 cm− 3, 7.83 cm2/V.s, and 1.64 × 10− 2 Ω.cm, respectively. The FoM is calculated as 1.27 × 10− 4 Ω−1. The electrical output parameters of the fabricated a-IGZO MSM UV photodetector were also evaluated, including responsivity, detectivity, noise-equivalent power, photo-to-dark current ratio, and the normalized photo-to-dark current ratio. The ultraviolet light exposure leads to a current increase of 6.375 µA. The critical voltage for the device is 3.02 V. The highest measured responsivity, 48.99 A/W, was measured at room temperature at the critical voltage. The maximum detectivity was found to be 4.37 × 1013 Jones under an applied bias of 0.79 V. The minimum NEP is 2.29 × 10− 13 W/Hz1/2 obtained at 0.79 V. The maximum PDCR and NPDR are observed at 0.14 V, corresponding to 31.207 and 9.202 × 106 W− 1, respectively. Responsivity, detectivity, noise equivalent power, photo-to-dark current ratio, and normalized photo-to-dark current ratio at the critical voltage are 12.72 A/W, 1.13 × 1013 Jones, 7.69 × 10− 13 W/Hz1/2, 0.386, and 3.96 × 105 W− 1, respectively. The results demonstrate that the a-IGZO MSM UV photodetector exhibits behaviors comparable to those reported in the literature for ultraviolet photodetectors, confirming the potential of a-IGZO as a promising material for advanced optoelectronic applications. In addition, this comprehensive study makes a significant contribution to the literature on a-IGZO MSM UV photodetectors, offering easy fabrication processes and low production costs. Electronic Supplementary Material Below is the link to the electronic supplementary material. Supplementary Material 1 Acknowledgements Thanks to the Director of the Photonics Application and Research Center, Prof. Dr. Süleyman ÖZÇELİK, and all members. Author contributions TARIK ASAR (TA): Writing – original draft, review & editing, Characterization, Investigation, Data Analysis, Editing. Funding This study was supported by the Gazi University Scientific Research Projects Coordination Unit (BAP) under the YÖK ADEP project, with project number FGA-2022-8034. Data availability The datasets used and/or analyzed during the current study are available from the corresponding author on reasonable request. Declarations Competing interests The authors declare no competing interests. Footnotes Publisher’s note Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations. References Associated Data Supplementary Materials Supplementary Material 1 Data Availability Statement The datasets used and/or analyzed during the current study are available from the corresponding author on reasonable request.