Fermi-level depinning achieved by high-work-function Au1-xSex alloy contacts for high-performance p-type WSe2 transistors Authors: Wanying Li, Yipu Xia, Yuanhao Kou, Hai Wang, Shaogang Xu, Yujia Deng, Chun Kit Ng, Tianyuan Chen, Sujuan Ding, Lin-Yun Huang, Fanqi Wei, Fangyuan Zheng, Ni Yang, Wanqing Meng, Chengdong Yao, Dong-Keun Ki, Xuming Zhang, Mingxin Huang, Hu Xu, Bo Wang, Chuanhong Jin, Junqiu Zhang, Maohai Xie, Lain-Jong Li Published: 2026 ABSTRACT AbstractP-type contact in two-dimensional (2D) transition metal dichalcogenides (TMDs) faces more severe Fermi-level pinning (FLP) than their n-type counterparts due to the damage caused by high-work-function metal deposition. Here, we demonstrate a simple molecular beam epitaxy (MBE) contact strategy using a high-work-function (5.8 eV) Au1-xSex alloy to achieve Fermi-level depinning in monolayer WSe2 p-type transistors. The Au1-xSex alloy mitigates both defect-induced gap states (DIGS) and metal-induced gap states (MIGS) by gentle pre-deposition of selenium (Se) followed by the conversion to Au1-xSex alloy by deposition of Au at low-temperature, forming a van der Waals (vdW) interface between Au1-xSex and monolayer WSe2. Moreover, it imposes hole doping to the contacted monolayer WSe2, reducing the Schottky barrier height and enabling favorable p-type device performance. Combined experimental and theoretical analyses confirm quasi-ohmic contact behavior, yielding a contact resistance of 492 Ω·µm, an on-current of 385 µA/µm, and an on/off ratio greater than 108 for a p-FET with a 100 nm channel length. This work establishes Au1-xSex alloy contacts as a scalable solution for high-performance p-type 2D electronics.Subject terms: Electronic devices, Electrical and electronic engineering Introduction The relentless scaling of silicon-based metal-oxide-semiconductor field-effect transistors (MOSFETs) has encountered fundamental limitations due to severe short-channel effects, including drain-induced barrier lowering (DIBL) and source-to-drain leakage current increase1. Two-dimensional materials such as transition metal dichalcogenides (TMDs), with their atomic-scale thickness and inherent electrostatic gate control, have emerged as promising candidates to extend Moore’s Law2–6. Great progress has been made on improving the performance of TMDs-based field effect transistors (FETs)7–9. Especially, n-type TMD FETs have achieved near-quantum-limited contact resistance (Rc) through low-melting-point metal contacts (e.g., In, Sb, Bi)10–12. However, p-type contact remains significantly hampered by Fermi-level pinning (FLP) failing to rival their n-type counterparts13–15. Achieving low Rc in p-type FETs necessitates high-work-function metals, which typically exhibit elevated melting points16–18. The deposition of such metals inevitably subjects atomically thin TMDs to high-energy bombardment, inducing defect-induced gap states (DIGS)12,19. For monolayer WSe2, a widely studied p-type TMD20, the presence of inherent Se vacancies in chemical-vapor-deposited films further aggravates DIGS21,22. Besides, when a metal forms an interface with a semiconductor surface, it introduces a distribution of electronic density of states (DOS) within the semiconductor bandgap known as metal-induced gap states (MIGS)11,23. These interfacial states exacerbate FLP, leading to substantial Schottky barriers (SBs) and degrading charge injection efficiency19,24. Recently, gas doping or introduction of band alignment layers have achieved good performance in p-type FETs25–30. However, satisfactory performance of p-type FETs has not yet been achieved without external doping or band engineering. Here, we demonstrate a simple contact engineering approach that simultaneously suppresses MIGS and DIGS by growing Au1-xSex alloy contact at low-temperature using molecular beam epitaxy (MBE) on metal organic chemical vapor deposition (MOCVD)-grown monolayer WSe2. Photoelectron spectroscopy (PES) and scanning tunneling spectroscopy (STS) studies confirm that the Au1-xSex alloy exhibits a high work function of 5.8 eV, enabling a low p-type SB height and quasi-ohmic contact, in consistence with density-functional theory (DFT) calculations. The deposition of Se at low sublimation temperature preserves the monolayer WSe2 lattice and protects it against high-energy Au bombardment during the subsequent Au deposition process, thereby reducing DIGS. A larger van der Waals (vdW) gap at the interface between the formed Au1-xSex alloy and WSe2 significantly suppresses MIGS. In our work, on-current of 385 µA/µm of p-type FETs is achieved on monolayer WSe2 film without any gas doping or additional intercalation layers. Our devices also have a near-ideal switching ratio of more than 108, and a contact resistance of 492 Ω·µm, marking a critical advancement toward scalable, high-performance p-type 2D electronics. Results and discussion Fermi level depinning by Au1-xSex alloy Before presenting the experimental results, we first show DFT calculations of the electronic structure of the proposed approach (see Methods for calculation details). Figure 1a displays the atomically projected band structure of 3-layer Au1-xSex in contact with a monolayer WSe2, where x = 0.10 for the specific model presented. Compared to the case of a pure Au contacted with WSe2 (Fig. 1b), the WSe2 exhibits a notable hole doping effect after made contact with Au1-xSex alloy. Specifically, as seen from Fig. 1a, the Au0.90Se0.10–WSe2 contact gives rise to a notable downward shift of the Fermi level (EF) towards the valence bands upon orbital hybridization, along with a diminishing DOS in the monolayer WSe2 energy gap. Band structures of models with different alloy compositions (x = 0.06, 0.10, 0.11, 0.25 and 0.33 in the contact layers) are presented in Supplementary Fig. 1. DFT calculations of changing alloy composition or changing the alloy layer thickness (Supplementary Fig. 2) do not reveal qualitive changes about the diminished metal-induced gap states and the hole doping effect. To elucidate the nature of band hybridization, we analyzed the projected density of states (PDOS) as shown in Supplementary Fig. 3 as well as the total DOS of the monolayer WSe2 near EF when it is in contact with Au0.90Se0.10 and Au (111), respectively (Fig. 1c, d). The calculations reveal pronounced MIGS within the bandgap and thus the propensity of FLP for the Au-WSe2 contact, whereas the alloy-WSe2 contact substantially suppresses interface states and leads to a FLP-free system. Besides, it promotes a p-type doping effect in the WSe2 monolayer. These findings show good agreement with our scanning tunneling microscopy/spectroscopy (STM/S) measurements shown in Fig. 1e and obtained from a monolayer WSe2/Au1-xSex sample flip transferred on Au using wafer bonder (see Methods and Supplementary Fig. 4 for more details). As seen from Fig. 1e, when the monolayer WSe2 is in contact with the Au1-xSex alloy, STS shows no obvious in-gap states, and the semiconductor shows a clear p-type behavior. Such a gap-state-free characteristic is similar to WSe2 on typical vdW substrates such as graphene31,32, indicating a very weak interaction at the interface. On the other hand, when the monolayer WSe2 is in contact with pure Au (111) (Fig. 1f), STS detects obvious gap-states originated from the relatively strong coupling between WSe2 and Au (111)33, and the semiconductor shows an unfavorable n-type behavior. To elucidate further the charge transfer characteristics, charge density difference calculations were carried out for both systems (Fig. 1g, h). Figure 1g clearly presents the interface charge depinning effect for the Au0.90Se0.10-WSe2 heterointerface, consistent with the above experiments and calculations. For such a model system, both the hybridization degree and charge transfer magnitude are significantly suppressed, suggesting improved vdW contact property. Bader charge analysis indicates a small electron transfer of ~2.98 × 10−5 e/Å2 from WSe2 to 3-layer Au0.90Se0.10, so p-type doping of the semiconductor is promoted in the system. This is consistent with our STS results that the Fermi level shifts towards the valence bands by ~0.5 eV when WSe2 is in contact with Au1-xSex alloy, compared to WSe2/Au, indicating a hole doping effect to monolayer WSe2. We also note, in passing, that according to our DFT calculations, a surface alloy layer is sufficient to cause MIGS-suppression and induce hole doping at the metal-semiconductor interface as presented in Supplementary Fig. 1. After all, the coupling and hybridization are dominated at the interface layers. Figure 1i, j schematically show the band alignment of WSe2 in Au1-xSex-WSe2 and Au-WSe2 configurations, illustrating effective mitigation of the FLP and induction of hole doping in WSe2 monolayer by contact with an Au1-xSex alloy. Electronic structures of Au1-xSex-WSe2 contact and Au-WSe2 contact. Density-functional theory (DFT) calculated energy bands of a, Au1-xSex –WSe2 contact (x = 0.10) and b, Au-WSe2 contact, where the bands from WSe2 monolayers and metals are highlighted in red and gray respectively (Fermi level set to 0). The size of the symbols represents the relative contribution. c, d DFT calculated density of states (DOS) of WSe2 monolayers in contact with c, Au1-xSex (x = 0.10) and d, Au, respectively. e, f Scanning tunneling spectroscopy (STS) spectra (mains) and atomic resolution scanning tunneling microscopy (STM) images (insets, sizes and sample biases: e 10 nm × 10 nm, −0.50 V and f 5 nm × 5 nm, 0.03 V) measured on WSe2 monolayers in contact with e, Au1-xSex and f, Au, respectively. The baselines of differential conductance were set to 0. g, h Stick-and-ball models with charge density difference of g, WSe2 monolayers on 3-layers Au1-xSex (x = 0.10) and h, on Au, where the W atoms, Se atoms and Au atoms are colored in gray, green and yellow respectively. The isosurface was set to 0.002 e/bohr3. i, j Schematic diagrams of the DOS as extracted from c and d on i, Au1-xSex and j, Au, where the metal induced gap states (MIGS) are illustrated in red color. CB and VB represent conduction bands and valence bands respectively. To guide the eye and facilitate comparison between the calculation and experimental results, red dashed lines are drawn across Fig. 1a–f to indicate the calculated conduction band minimum (CBM) and valence band maximum (VBM), while the gray dashed lines mark the Fermi levels. MBE growth of Au1-xSex alloy and Characterization For device purposes, we fabricate the Au1-xSex-WSe2 contact using MBE according to the following procedure: the MOCVD-grown WSe2 films were transferred on a dielectric (HfO2) and loaded into MBE. Se films of ~3 nm thick were then deposited at a low-temperature (~−140 °C). The low substrate temperature ensured more uniform Se films covering fully the WSe2 monolayer. Deposition at room or higher temperatures resulted in severe clustering of Se, prohibiting the full coverage of WSe2 by Se (refer to Supplementary Fig. 5). In addition, low-temperature would alleviate lattice damage of WSe2 by the deposit16,34. Upon the completion of Se-film deposition, Au film was deposited at temperatures below −120 °C for a thickness of about 30 nm, after which the sample was warmed up slowly to room temperature over a period of around 2 h. Such a deposition procedure is found to produce the desired Au1-xSex contact film on WSe2 according to an array of experimental characterizations and theoretical investigation. Indeed, the propensity of Se to alloy with Au can be inferred by our ab initio molecular dynamics (AIMD) simulation results (refer to Supplementary Fig. 6), which shows that even for a stable Se (0001)-2×1 structure35, the deposited Au atoms readily displace Se atoms and dive in crystal, forming an alloy with Se. Experimentally, formation of an Au1-xSex alloy are evidenced by X-ray photoelectron spectroscopy (XPS), energy dispersive X-ray spectroscopy (EDS), three-dimensional atom probe tomography (3D-APT), electron energy loss spectroscopy (EELS), X-ray diffraction (XRD) and scanning transmission electron microscopy (STEM) measurements. The comparison of concentration estimates by 3D-APT, XPS and EDS, along with their respective characterization advantages, are summarized in Supplementary Fig. 7. Cross-sectional annular dark-field STEM (ADF-STEM) experiments were carried out on such samples. Figure 2a, b present typical results, which reveal the atomic structure of an Au1-xSex alloy interfaced with WSe2. Since Se and Au show minimal contrast difference in cross-sectional STEM (refer to Supplementary Fig. 8 for abTEM simulated images), these micrographs unfortunately do not provide direct evidences about the atomic configuration in the alloy. However, by the homogeneity and regularity of the lattice, we suggest Se incorporation is predominantly substitutional rather than interstitials. In fact, according to our abTEM simulations, if Se occupies interstitial sites, pronounced lattice distortion and intensity variation would be shown in STEM, which we have so far failed to detect. Besides, our DFT calculations also suggest that the substitutional configuration is more energetically favorable than interstitials (Supplementary Fig. 8). In any case, the alloy film exhibited an expanded lattice according to STEM measurements. By averaging over 500 atoms in the STEM micrographs (Supplementary Fig. 9), we estimate a lattice constant of about 4.3 Å of the alloy film, which is markedly larger than that of a pure gold film deposited directly on WSe2 without the Se buffer (~4.1 Å). An expanded lattice was also verified by XRD measurements (Supplementary Fig. 10). The EELS characterizations of the contact film in the electron microscope (Supplementary Fig. 11) reveal the characteristic Se L-edge together with the Au M-edge, affirming the co-existence of Au and Se, indicating an Au1-xSex alloy. From STEM micrographs, one further notes that the alloy and WSe2 monolayer forms a sharp interface without Se residual (see, e.g., Fig. 2b), and a weakened coupling between WSe2 and Au1-xSex than that with Au may be inferred by an enlarged vdW gap that is measured to be about 2.5 Å for the case of Au1-xSex-WSe2 but 2.2 Å for the Au-WSe2 contact (see Supplementary Fig. 12). The STEM allowed us to cross check the chemical distribution profile in the sample by an elemental energy-dispersive X-ray spectroscopy (EDS) mapping and spectrum analysis as shown in Supplementary Figs. 13 and 14, again revealing a dispersed Se distribution profile throughout the Au contact layer. Separately, an independent 3D-APT measurement of a similar sample as shown in Fig. 2c provides additional direct and unambiguous evidence for the presence of Se dispersed over the film, suggesting it is an alloy of Au and Se rather than a pure Au film, and the estimated average Se content is at ~6%. Characterizations of Au1-xSex-WSe2 contact. a Annular dark-field scanning transmission electron microscopy (ADF-STEM) image of the cross-section of WSe2 in contact with Au1-xSex. Scale bar, 2 nm. b Zoom-in atomic-resolution STEM image with schematic model, where W (gray), Se (green) and Au (orange) atoms are overlayed on the image. The vdW heterointerface gap is 2.5 Å wide as marked. Scale bar, 1 nm. c 2D slice view of three-dimensional atom probe tomography (3D-APT) analysis of the alloy film, showing Se and Au (colored in blue and yellow, respectively) distribution over the analyzed region. d, e X-ray photoelectron spectroscopy (XPS) characterizations of Au1-xSex, Au, and Se films, and in e, peak fitting results are also shown. f Ultraviolet photoelectron spectroscopy (UPS) spectra of Au1-xSex and Au(111). Figure 2d, e shows typical XPS spectra of Au1-xSex alloy, which reveal a binding energy shift of the Au 4f peaks to a higher value by ~ 0.2 eV when compared with that of the bulk Au (Fig. 2d). For the Se 3d orbitals (Fig. 2e), fittings of the broader and shouldered peak resolve the Se 3d3/2 and Se 3d5/2 peaks that are red-shifted by ~ 0.2 eV in the Au1-xSex alloy than that of a MBE-grown Se film of ~20 nm thick, conforming to the bonding characteristics between Au and Se36,37. We remark that the Se peak in Fig. 2e is unlikely from WSe2 embedded in the sample, since the top Au1-xSex layer is ~30 nm thick and the measured spectrum contains no signal of W (Supplementary Fig. 15). These results suggest that Se are incorporated in Au with chemical bonding, i.e., in the form of an alloy, rather than physical mixtures or surface adsorbates. Presented in Supplementary Fig. 16 are a series of XPS results obtained at varying depths of the film by argon sputtering. It consists of 24 sputtering/probing cycles of a grown Au1-xSex/WSe2 sample (see Method). The existence of Se in the metal film can be clearly noted, where the composition estimated through peaks fitting varies between 8% to 11% across the entire thickness. To further attest the alloy, ultraviolet (UV) visible spectrum of the Au1-xSex alloy film is acquired and shown in Supplementary Fig. 17 and compared with that from pure Au and Se films. It reveals differences as well as shift of the absorption peaks, inferring certain interaction between the Se atoms with the surrounding Au atoms to lower the band energy, suggesting an alloy than mixtures of Au and Se. Finally, ultraviolet photoelectron spectroscopy (UPS) experiments were also carried out in situ, i.e., in a chamber vacuum interlocked with the MBE reactor immediately after the sample was grown and transferred without exposing to air. The UPS spectra shown in Fig. 2f for the Au1-xSex-WSe2 and Au-WSe2 samples reveal a work function difference, ~5.8 eV for the alloy and ~5.2 eV for pure Au. The spectrum and consequently the work function of Au1-xSex alloy exhibit no change after in situ annealing at 300 °C for 2 h (Supplementary Fig. 18), suggesting firstly good thermal stability of the alloy film and secondly the spectrum is characteristic to the alloy rather than from possible surface Se contaminates, as annealing would have effectively desorbed the adsorbates, if present at all. Notably, the work function of the alloy is significantly larger than pure Au, suggesting an appealing candidate for making p-type contact with monolayer WSe238. At this juncture, we wish to make a comment on the possible pathway under which the alloy is formed upon Au deposition on a thin pre-deposited Se film at low-temperature. Firstly, we remark that possible background Se or those evaporated from the walls of the MBE reactor acted as the source of alloy growth is ruled out, since depositing Au under the same condition but directly on WSe2 without the Se buffer layer has been found to lead to a pure Au film (Supplementary Figs. 9 and 10). In other words, the alloy must have formed by consuming the pre-deposit Se layer, which is consistent with the STEM observation that the Se layer has vanished after the Au deposition (see, e.g., Fig. 2a and b). To evaluate possible processes, we performed AIMD simulations (Supplementary Fig. 6), which showed that for the (2 × 1) surface reconstructed crystalline Se (0001)35, it remained stable at both room-temperature (300 K) and 150 K after 650 ps. When adsorbed with Au, the Se film became decomposed, and Se atoms were desorbed after 650 ps at 300 K. At the low-temperature (150 K), however, although Se atoms were also displaced, they remained in film, leading to a net effect of Au incorporation in Se. Therefore, low-temperature appears critical in order to maintain the needed Se for alloy formation, consistent with the experiments. Low-temperature also ensures Au and Se are locally trapped, prohibiting bulk diffusion or migration of atoms into pure Se and Au phases, which would otherwise be favorable due to low solubility. Based on the above, we may postulate a process as follows (Supplementary Fig. 19), but also note that it remains speculative and more systematic studies are needed to establish firmly the underlying mechanism of Au1-xSex alloy formation: after a uniform ~3 nm thick Se film is deposited on the monolayer WSe2 at low-temperature, Au is deposited from high-temperature cells, which possesses high kinetic energies capable of displacing Se and dives deeper into the Se film before becoming equilibrated with the sample temperature (150 K) and trapped inside, forming the alloy with Se. Expectedly, an optimal Se film thickness exists: too thick a film will make the Au atoms unable to reach to the very bottom of the Se layer, so besides an alloy, a residual of pure Se would remain at the interface, which is evidenced experimentally (Supplementary Fig. 20). If the Se film was too thin, the Au atoms would retain the high kinetic energy even after reaching the Se-WSe2 interface, causing damages to WSe2. Experimentally, an optimal Se film thickness about 3 nm has been identified. The Se pre-deposit layer thus not only serves as the source needed for growing the Au1-xSex alloy, but it also plays the role of protecting the WSe2 monolayer underneath, mitigating the effect of lattice damage of WSe2 by the high energy Au atoms from source cells39,40. As a result, an atomically sharp, damage-free, interface is achieved. Together with the high chemical purity inherent to the MBE-grown films, this gives rise to an electronically clean interface and depinned Fermi level, desirable for good ohmic metal-semiconductor contacts. This contrasts the Au-WSe2 contact, where structural damage in monolayer WSe2 is revealed by STEM (Supplementary Fig. 21). Recently, adopting semiconducting selenium interfacial contact layers for WSe2 were reported41,42. They contrasted to our approach where an Au1-xSex alloy contact was generated and stabilized by low-temperature MBE growth. As described above, when we had an excess Se being deposited prior to Au deposition, some Se residuals would be maintained at the interface, creating a similar contact structure as in the above mentioned papers41,42. Electrical properties of Au1-xSex contact We now turn to evaluate the electrical properties of the Au1-xSex contact by measuring p-type FETs using the MOCVD-grown monolayer WSe2 films as the channel on a 6 nm-thick hafnium dioxide (HfO2) high-κ dielectric (see Methods for fabrication and measurement details). Figure 3a presents the transfer characteristics (drain current Id – gate voltage Vg) of the monolayer WSe2 FET with Au1-xSex contact at drain-to-source voltage (Vds) = 1.0 V and 0.1 V (channel length Lch = 100 nm). Note that for p-type transistor operations, a reverse bias polarity is conventionally applied. We therefore show in Supplementary Fig. 22 the transfer characteristics of the device for both positive and negative biases at small and large Vds for comparison. In any case, the devices exhibit excellent short-channel immunity with negligible drain-induced barrier lowering. A high on-current (Ion) of 385 μA/μm at Vds = 1.0 V, an on/off ratio exceeding 108, and a subthreshold swing (SS) of ~220 mV/dec has been achieved. The Ion value of 385 μA/μm surpasses the reported values for conventional metal contacts (e.g., Pt, Pd16) and vdW Au with selenide buffer39. Notably, the device performance retains after overnight annealing at 160 °C and 1 h annealing at 240 °C without degradation, suggesting good thermal stability of the device (Supplementary Fig. 23). Figure 3b displays the linear output characteristics (Id–Vds) of the same FET (Lch = 100 nm) for gate voltages (Vg) ranging from −1.6 V to −3.4 V in −0.2 V steps. The device demonstrates robust saturation behavior at Vds = −1.2 V, corroborated by both the transfer and output curves. Carrier mobility of the device was extracted from a long channel (Lch = 1000 nm) device from the linear region of the transfer characteristics (see Supplementary Fig. 24), which amounts to ~43 cm2V−1s−1, indicating a high-quality channel material (WSe2) of the device. The transfer curves under full gate bias are shown in Supplementary Fig. 25a and the devices exhibit ambipolar behavior. The pristine WSe2 is intrinsically ambipolar and its Fermi level lies in the middle of the band gap without extrinsic doping or Fermi-level pinning. Although our Au1-xSex contacts have a relatively high work function of 5.8 eV, which would be an ideal p-type contact, a positive gate bias can still shift the Fermi level toward the conduction band, and therefore induce n-type current. The n-branch current will be suppressed by employing doping techniques such as NO and O₂ annealing in our future work. Electrical characteristics of Au1-xSex contact 1L-WSe2 device. a Transfer curve of typical Au1-xSex - monolayer WSe2 contact with Lch = 100 nm under Vds = 1.0 V (blue line) and Vds = 0.1 V (pink line). Lch is the channel length, Vg is the gate voltage, Vds is the drain-to-source voltage, and Id is the drain current. b The output performance of the same device in a, for different gate voltage Vg ranging from −1.6 V to −3.4 V with −0.2 V step intervals. c Total resistance (Rtotal) as a function of Lch. The transfer-length-method (TLM) method is used for contact resistance (Rc) extraction. Inset: Boxplots of total resistance as a function of Lch for 6 TLM sets. The boxplot statistics were performed, showing mean (spot symbols), standard deviation, lower quartile (25%), median (50%), upper quartile (75%), interquartile range (25–75%). d Transfer curves of a typical TLM structure with Lch ranging from 0.1 μm to 1.5 μm and Vds = 1.0 V. Inset: scanning electron microscope image of a TLM structure. Scale bar, 2 μm. e Id–Vg of Au1-xSex –WSe2 at various temperatures from 300 K to 30 K. Inset: Zoom-in view of the transfer curves at Vg ranging from −4.0 V to −3.4 V. f Benchmark of Id vs. Lch of state-of-the-art contact approaches of WSe2 p-FETs without doping, Id at Vds = 1.0 V16,26,39,41,44–48. To highlight the superior contact properties of Au1-xSex alloy, we conducted a performance comparison with direct Au metal contact configurations. As shown in the transfer characteristics in Supplementary Fig. 25, the typical Au1-xSex alloy layer as a band-aligned contact exhibits optimal electrical performance. As discussed earlier, the Se film forms a wetting layer at low-temperature and protects the surface of 2D TMDs. For direct Au contact with WSe2, high-energy Au atoms during deposition cause significant damage, inducing DIGS as shown in Fig. 1f, which limits the on-current to the microampere level, consistent with literature reports40. Clearly, the Au1-xSex alloy aligns closely with the VBM of WSe2, facilitating efficient hole injection for the p-branch. We also compared the device performance made from a contact film by depositing Au on a thicker Se buffer layer that has caused non-uniform Se residual as shown in Supplementary Fig. 25. Though the device performance is inferior compared to Au1-xSex alloy contact, it still demonstrates better performance than direct Au contacts. The transfer-length-method (TLM) analysis43 from a particular device set is shown in Fig. 3c, which reveals a contact resistance (Rc) of ~492 Ω·µm for the Au1-xSex-WSe2 contact, consistent with the formation of clean vdW interface and the absence of Fermi-level pinning. Data from six sets of the TLM devices are shown in the inset with an average Rc of ~813 Ω·µm. Figure 3d compares the transfer performances across channel lengths (Lch = 100-1500 nm) measured via TLM devices, with an inset showing the corresponding SEM image (channel width = 1.0 μm). When the temperature is lowered from room temperature (300 K) to 200 K, the drain current increases significantly as shown in Fig. 3e. From 200 K to 77 K, we observe a slight current attenuation. This phenomenon can be attributed to the competition between phonon scattering and thermionic emission mechanisms. In the range of 300 K to 200 K, thermionic emission of holes is sufficient to overcome the SB height, and phonon scattering dominates the transport behavior. The reduction in temperature significantly suppresses lattice scattering, leading to an increased hole mean free path and consequently enhanced current. However, when the temperature further decreases to below 200 K, the weakening of thermionic emission becomes the dominant limiting factor due to the presence of a small Schottky barrier, resulting in the observed current attenuation. Even when cooled to 30 K, the Au1-xSex-WSe2 contact device maintains a linear output curve (see Supplementary Fig. 26). This observation indicates that the ohmic contact is not yet perfect and a small SB height remains. In Fig. 3f, we have benchmarked the Id vs. Lch performance of our devices against the best-reported p-type 2D TMD transistors employing various contact strategies. Our devices display a high current at 100 nm channel length16,26,39,41,44–48 than the previous record in p-type WSe2 solely through the evaporation method. Notably, while the best-performing devices in prior reports were typically based on multilayer (2 or 3 L) channels, our devices employ monolayer WSe2, which is more challenging to optimize, yet still achieve performance comparable to state-of-the-art multilayer devices. Furthermore, when compared with state-of-the-art p-FETs utilizing doping techniques, our devices still demonstrate strong competitiveness (refer to Supplementary Fig. 27)13,25,27–29,41,49,50. Lastly, to validate the excellent uniformity and scalability of Au1-xSex-WSe2 contact p-FETs for large-scale integration, we fabricated 75 devices with varying channel lengths Lch and characterized their transfer characteristics, as shown in Fig. 4a. Statistical analysis of key device metrics reveals significant performance enhancement through channel length scaling. The statistical distributions of Ion, Vth, and SS as functions of channel length are systematically as quantified in Fig. 4b–d. The on-current Id increases from an average of 30 µA/µm to 200 µA/µm at Vg = −4.0 V with reducing Lch from 1000 nm to 100 nm. While some device-to-device variation is observed (attributed to batch-to-batch differences and WSe2 film quality variations), the consistent Ion improvement with scaling confirms the devices remain non-contact-limited, further evidencing the low contact resistance. Notably, the threshold voltage remains stable across scaled channels, while the subthreshold swing shows only minor degradation at Lch = 100 nm. This is a signature of short-channel effects likely originating from non-optimized 2D semiconductor/high-κ dielectric (HfO2) interfaces. Variability of Au1-xSex contact 1L-WSe2 p-type field effect transistor (p-FETs). a Transfer characteristics of Au1-xSex–WSe2 p-FETs with channel lengths of 100 nm, 400 nm, 600 nm, 800 nm and 1000 nm under Vds = 1.0 V. b–d Boxplots of key device metrics, including on-current (Ion), threshold voltage (Vth), and subthreshold swing (SS). The color of the symbols corresponds to the channel length in a. For each group of data, the boxplot statistics were performed, showing mean (cross symbols), standard deviation, lower quartile (25%), median (50%), upper quartile (75%), interquartile range (25-75%). In summary, we developed a Au1-xSex alloy contact strategy that overcomes Fermi-level pinning and defect-related challenges in p-type monolayer WSe2 transistors. The high work function (5.8 eV) and low-energy deposition process preserve the WSe2 lattice integrity. Through DFT calculations and STS measurements, we verified the suppression of interfacial gap states and a van der Waals gap of 2.5 Å, enabling quasi-ohmic contact with a low Schottky barrier. Devices exhibited low Rc (492 Ω·µm), high on-current (385 µA/µm), and high switching ratios (>108), outperforming conventional metal contacts. Statistical analyses confirmed excellent uniformity across scaled channel lengths (100–1000 nm), highlighting the approach’s viability for large-scale integration. This study provides a generalizable framework for contact engineering in 2D semiconductors, advancing the development of energy-efficient, post-silicon electronics. Methods STM/S STM and STS measurements were conducted in a Unisoku 1500 STM system at ~77 K and under the base pressure of ~1 × 10−10 Torr. Constant current mode was used during scanning and the tunneling current was 100 pA. Tungsten tips were calibrated on clean Ag(111) surfaces before scanning. Flipped Au1-xSex/WSe2 sample by wafer bonder was specially prepared for purposes of the STM/S measurements: a bulk Au(111) single crystalline substrate and Au1-xSex/WSe2/sapphire were placed on the top and bottom platens of the wafer bonder with Au1-xSex facing Au(111). After bonding, the Au1-xSex/WSe2 is flip-transferred onto the Au substrate with the top layer being WSe2. For comparison, WSe2 grown on clean Au surface without depositing Se layer was also made. After the samples were loaded into the standalone Unisoku 1500 STM system, they were gently annealed at ~100 °C for 10 min, aiming to desorb any surface adsorbates or contaminates, if any. STEM characterizations Atomic-resolution ADF-STEM were performed in a probe-corrected TEM (FEI Titan Chemi STEM G2) operated at 200 kV. The convergence semi-angle was set at 21.4 mrad and the range of acceptance angle of the ADF detector was 53–200 mrad. Cross-sectional STEM specimen was prepared via the focused ion beam (FIB) technique (FEI Helios G4), during which cares like coating of amorphous carbon and platinum as protected layers and low-voltage polishing at 5 kV (48 pA current) were taken to minimize sample damage. UPS and XPS In situ UPS measurements were carried out in a separate UHV chamber vacuum-interlocked with the MBE. The base pressure was in the 10−10 mbar range. Samples after the MBE growth were transferred directly to the analysis chamber without exposure to air and any additional treatment. For the UPS, a high intensity helium discharge lamp (He-I = 21.22 eV) was used, photoelectrons were analyzed by SPECS PHOIBOS 100 MCD−5 electron analyzer. XPS measurements were performed ex situ together with argon sputtering for depth profiling in an Escalab QXi system Electron Microscope Unit (EMU) of HKU University Central Facilities. Each etching cycle by argon sputtering operated at 1000 V lasted for 10 s, which was estimated to etch away ~1.4 nm of the film, XPS measurement then followed. Such a sputtering/probing cycle was repeated until the WSe2 film was reached as indicated by the emergence of W-related peaks in the spectra. 3D-APT A dual-beam focused-ion-beam was used to prepare the atom probe samples. Annular milling with acceleration voltage of 30 kV was used to mill the samples into sharp tips. Cleaning steps with a lower acceleration voltage at 5 kV were applied to reduce Ga ion damage on the sample from the ion beam. Atom probe analyses were performed in a Cameca LEAP 6000XR system, using laser mode acquisition. The parameters used are as follows: laser energy at 25pJ, laser pulse rate at 100 kHz, detection rate at 0.15–0.2% per pulse, sample temperature at 50 K. Data analysis was performed using the AP Suite software (version 6.3) from Cameca. DFT The first-principles calculations were performed based on density functional theory (DFT) as implemented in the Vienna ab initio simulation package (VASP)51. The electron-ion interactions were described by the projector augmented wave (PAW) potentials52. The exchange correlation functional was treated using the Perdew−Burke−Ernzerhof (PBE) generalized gradient approximation (GGA)53, with a plane wave kinetic energy cutoff of 480 eV. In order to ensure accurate convergence results, the k-point sampling parameters were tested and chosen following the Monkhorst–Pack scheme54. The substrates of the slabs were constructed by five atomic layers with the bottom two Au layers fixed, and a vacuum space of 18 Å was introduced along the z-axis to eliminate periodic interactions. The interfacial interactions of the WSe2-metal junctions were treated by the DFT-D3 correction in Grimme’s scheme55. All initial slab models were fully relaxed until forces on each atom were smaller than 0.02 eV Å−1, and the energy convergence criterion was 10−5 eV. However, in calculating the 3 L Au1-xSex /WSe2 system, restricted relaxation along lateral direction was applied, where the relaxed atomic structure matches better the experimental observations. To demonstrate that Au atoms can easily penetrate the Se crystal, we employed ab initio molecular dynamics (AIMD) simulations with a Nosé heat-bath scheme56 at room temperature. Visualization of the charge density difference was accomplished using VESTA software57. Device fabrication For p-FETs fabrication, the local back gate composed of a Ti (3 nm)/Au (12 nm) metal was defined using electron-beam lithography (ebl), and then 6 nm HfO2 layer was deposited via atomic layer deposition (ALD) at 180 °C to serve as the gate dielectric. Monolayer MOCVD-grown WSe2 film was transferred onto the dielectric using a standard PMMA assisted DI-water delamination method by thermal-release tape. Briefly, PMMA was spin-coated and baked on the as-grown monolayer WSe2 on sapphire. A thermal-release tape (TRT) layer was then laminated on top. The stack was subsequently floated on DI water, which allowed the TRT/PMMA/WSe2 film to delaminate from the sapphire, and the film was then transferred onto the HfO2/local back gate substrate with the local back-gate. Finally, TRT was released at 110 °C and PMMA was removed in acetone and IPA. The channel area was defined as width of 1 μm using ebl and reactive ion etching (RIE) at 30 mTorr and 30 W. After annealing at 350 °C for 2 h with Ar/H2 to remove residuals, ebl was employed again to define Au1-xSex/Au source/drain (S/D) contacts. MBE evaporation Growths of Au1-xSex contact on monolayer WSe2 were carried out in an Omicron MBE system having the background pressure of low 10−10 Torr. The samples were cooling down to around −140 °C before growth. The fluxes of Se and Au were generated from Knudsen cells held at ~125 °C and ~1240 °C, respectively. Se was firstly deposited onto the sample for 25 mins, followed by Au deposition for ~90 mins at temperatures below −120 °C. In between the two deposition processes, growth was interrupted for periods ranging from hours to days, where the long period of interruption was to ensure effective pumping of background Se. Our experiments showed no significant difference, ruling out the background Se effect. This is presumably because the whole MBE chamber, source cell shroud and sample manipulator were all cooled by liquid nitrogen during deposition. The sample was only gradually warmed up to room-temperature (within ~120 min) after the completion of deposition. Electrical measurements Electrical characteristic measurements were performed at a Lakeshore probe station at room temperature under vacuum (~10⁻⁶ Torr) using an Keysight B1500A semiconductor parameter analyzer. Supplementary information Supplementary Information Transparent Peer Review file Acknowledgements L.L. thanks Nexstrom Singapore for providing WSe2 samples. The authors at ZJU thank the Center for Electron Microscopy of Zhejiang University for the access to Cs-corrected STEM. Author contributions L.-J.L., M.X., and Y.X. coordinated and supervised the project. W.L. and Y.X. conceived and directed the project. Y.X. carried out the MBE growth of metal contacts, W.L. and H.W. conducted electrical measurements and analyses of devices. L.-Y.H. synthesized the WSe2 monolayer. Y.K., B.W., S.D. and F.Z. conducted the FIB/TEM/STEM characterizations. Y.X. and Y.D. carried out PES characterization. W.L., Y.X., H.W. and Y.D. contributed to the device fabrication. J.Z. executed STM/S measurements. S.X. contributed to the DFT simulation. C.N. conducted the 3D-APT measurements under the supervision of M.H. J.Z. and C.Y. conducted the sample transfer by wafer bonder. F.W. conducted the UV spectra measurements under the supervision of X.Z. W.M., N.Y., C.Y., T.C., D.-K.K., M.H., H.X. and C.J. provided constructive opinions and suggestions. W.L, Y.X., H.W. and M.X. co-wrote and revised the manuscript with input from all authors. All authors discussed the results and commented on the manuscript. Peer review Peer review information Nature Communications thanks Jianfeng Jiang, Gihyeon Kwon, Yuxuan Cosmi Lin, and the other, anonymous, reviewer for their contribution to the peer review of this work. A peer review file is available. Funding L.L. thanks the support from National Research Foundation Singapore Professorship (NRF-P2025-002). M.X., Y.X. and J.Z. acknowledge the support by the Research Grant Council of Hong Kong SAR (AoE/P-701/20 and 17300925). J.Z. and M.H. acknowledge the support by the Research Grant Council of Hong Kong SAR (T46-705/23-R), J.Z. also acknowledges the HKU seed fund for basic research. S.X. acknowledges the National Natural Science Foundation of China (12204224) and Guangdong Basic and Applied Basic Research Foundation (2026A1515010017). M.X. and Y.X. acknowledge the support from Guangdong Provincial Quantum Science Strategic Initiative (No. GDZX2301003) and State Key Laboratory of Optical Quantum Materials. Data availability Relevant data supporting the key findings of this study are available within the article and the Supplementary Information file. All raw data generated during the current study are available from the corresponding authors upon request. Competing interests The authors declare no competing interests. Footnotes Publisher’s note Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations. These authors contributed equally: Wanying Li, Yipu Xia. Contributor Information Yipu Xia, Email: xiayp@hku.hk. Maohai Xie, Email: mhxie@hku.hk. Lain-Jong Li, Email: lance.li@nus.edu.sg. Supplementary information The online version contains supplementary material available at 10.1038/s41467-026-74149-y. References Associated Data Supplementary Materials Supplementary Information Transparent Peer Review file Data Availability Statement Relevant data supporting the key findings of this study are available within the article and the Supplementary Information file. All raw data generated during the current study are available from the corresponding authors upon request.