RSM optimized mechanical performance and chemical durability of nano silica, nano alumina fiber reinforced alkali activated mortar Authors: Mahmood Hunar Dheyaaldin, Mohammad Ali Mosaberpanah, Dler H Kadir, Gökhan Kaplan, Mustafa Özakça Published: 2026 ABSTRACT AbstractThis study aims to optimize the mechanical performance, durability, and environmental sustainability of alkali-activated mortars (AAM) incorporating nano-silica (NS), nano-alumina (NA), and polypropylene fiber (PPF). A three-factor, three-level Central Composite Design (CCD) within the Response Surface Methodology (RSM) framework was employed, generating 17 experimental mixtures prepared using fly ash (FA) and ground granulated blast-furnace slag (GGBS) as binder materials. The maximum compressive strength of 82 MPa was achieved in the mixture containing 2% NA, while the maximum flexural strength (12 MPa) was recorded in the mixture containing 1% NS and 0.5% PPF. ANOVA results confirmed the statistical significance of the developed models, with R² = 0.984 and R² = 0.977 for compressive and flexural strength, respectively. Nano-alumina produced a greater increase in strength than NS, and the combination of both nanomaterials enhanced the density of the microstructure through the formation of C-(A)-S-H and N-A-S-H gels. The incorporation of PPF improved durability by preventing microcrack formation and enhancing resistance to acidic and saline environments. For example, specimens containing 2% NS and 2% NA demonstrated more than 20% higher residual strength under sulfuric acid exposure compared with reference specimens. Scanning Electron Microscopy (SEM) analyses showed that the nanomaterials accelerated early strength development by filling micro-voids and creating a more homogeneous matrix structure. A CO₂ emission analysis indicated that the optimized AAM mixture emits approximately 607.4 kg CO₂/m³, representing a reduction of about 26%. The results demonstrate that alkali-activated mortars provide a strong and environmentally sustainable alternative to conventional cement-based systems, highlighting the efficiency and practical potential of this approach.Keywords: Alkali-activated mortar, Nano-silica and nano-alumina, Polypropylene fiber reinforcement, Response Surface Methodology (RSM), Low carbon construction materialsSubject terms: Engineering, Environmental sciences, Materials science Introduction Robust campaigns are being undertaken to promote sustainable living practices and to develop technologies that reduce carbon emissions. Reducing CO₂ emissions and limiting natural resource consumption are crucial strategies for producing durable and environmentally sustainable materials and products1. An international organization has proposed a four-step strategy to mitigate CO₂ emissions in the cement and concrete industry: (1) implementing advanced technologies in cement plants, (2) improving thermal and electrical efficiency, (3) replacing fossil fuels with sustainable alternatives, and (4) adopting carbon capture and clinker substitution technologies2. The pioneering work of Davidovits in the 1970s played an important role in advancing sustainable construction. He developed a special type of binder that produces significantly lower CO₂ emissions. This work demonstrated that high-quality and environmentally friendly concrete can be produced using alternative binder systems3. Similar materials, referred to as soil-cement, were used in the Soviet Union from the 1950 s, although their chemical compositions have evolved considerably since that time4. Most geopolymer compositions rely on liquid alkaline components and an aluminosilicate source5. Alkaline solutions activate aluminosilicate materials, forming a strong three-dimensional network structure. This process involves a chain reaction between aluminosilicate polymers and the alkaline solution, often under heat, resulting in geopolymer concrete, a sustainable binder comparable to traditional cement6,7. To improve flexibility, post-cracking behavior, and tensile performance, fibers are commonly incorporated into geopolymer matrices. PPF, in particular, helps prevent early-stage cracking by bridging microcracks, thereby increasing tensile strength and long-term durability8. The primary factor driving the ongoing climate change crisis is the significant increase in the concentration of various greenhouse gases (GHGs) in the atmosphere, particularly carbon dioxide9. Many countries are already experiencing the effects of climate change. Consequently, governments must collaborate to reduce greenhouse gas emissions; however, current efforts remain insufficient to curb the rapid growth of these emissions. To address this challenge, researchers have developed geopolymer concrete (GPC). Geopolymers are produced from materials rich in silica and alumina, such as fly ash (FA), metakaolin, and ground granulated blast-furnace slag (GGBFS or GGBS). These materials are often low-cost resources or industrial by-products (IBPs), making them a more sustainable alternative for construction applications10–13. These industrial by-products can serve as concrete binders when GGBS is activated using a high-pH alkaline solution. Geopolymer cement can be produced by activating GGBS with alkaline solutions such as sodium hydroxide (NaOH) and sodium silicate (Na₂SiO₃)14. Fly ash possesses important chemical constituents such as silicon dioxide (SiO₂), aluminum oxide (Al₂O₃), iron oxide (Fe₂O₃), and calcium oxide (CaO). In addition, trace amounts of titanium, potassium, magnesium, sodium, and sulfur compounds are present. According to ASTM International standards, the most commonly used types of fly ash are Class F and Class C. Class F fly ash differs from Class C fly ash in that it contains lower calcium oxide content, whereas Class C fly ash contains higher CaO levels. In some cases, Class C fly ash may contain up to 18% CaO15. The two most widely used alkaline activator solutions are sodium hydroxide and sodium silicate, and most studies assume that fly ash contains a significant amount of aluminosilicate compounds16,17. Fly ash can also be categorized as low-calcium or high-calcium fly ash. Compared with high-calcium fly ash, low-calcium fly ash typically contains approximately 80% silicon (Si) and aluminum (Al) by weight6,18. In certain countries, FA can be 20–60% less expensive than ordinary Portland cement (OPC), whereas in other cases OPC may be nearly twice as expensive as FA19. To ensure that molten slag forms a glassy phase and produces granulated blast furnace slag with cementitious properties, it must be rapidly quenched with air or water. Water quenching, particularly using high-pressure water jets, is generally considered the most effective method because it produces a higher proportion of glassy structures in the slag20. A by-product of iron and steel production, steel slag primarily consists of iron oxide, silicon dioxide, aluminum oxide, and calcium oxide. Trace amounts of sulfur trioxide (SO₃), titanium dioxide (TiO₂), and potassium oxide (K₂O) may also be present. Steel slag is generated during iron production in a basic oxygen furnace (BOF) and during steel production from scrap in an electric arc furnace. In a BOF process, impurities such as silicon, carbon, phosphorus, and manganese are removed using oxygen, forming slag when these elements combine with lime and dolomitic lime21. With its high silicate and alumina content, GGBS complies with ASTM C989, which allows the material’s properties to gradually evolve and improve over time22. The compressive strength of alkali-activated mortar generally increases during the curing period, with contributions from NA, NS, and PPF. Notably, specimens containing 1% NA and an appropriate NS content performed better than those without these nanomaterials13,23. Studies have shown that adding nano-silica in different proportions significantly enhances the compressive strength of FA and GGBS-based geopolymer mortars. For example, incorporating nano-silica in the range of 0–2% by weight in FA/GGBS geopolymer mortars has resulted in noticeable improvements in compressive strength. Nano-SiO₂ and nano-Al₂O₃ enhance the mechanical and durability properties of geopolymer systems by filling micro-voids, refining the pore structure, and promoting additional gel formation24. These highly reactive silica particles can also act as micro-fillers between binder materials and aggregates in FA and GGBS-based geopolymer concrete25. Nanomaterials such as nano-alumina (Al₂O₃) and nano-silica (SiO₂) have been reported to increase the shear bond strength between the concrete substrate and geopolymer matrix26. When combined with PPF, these nanomaterials create a synergistic effect that simultaneously enhances compressive strength, flexural toughness, and resistance to chemical attack, an interaction that has not been thoroughly explored in previous studies27. Sodium hydroxide plays a critical role in geopolymer reactions and significantly influences the structure and compressive strength of geopolymers. The concentration of NaOH in the aqueous phase of the geopolymer system affects the dissolution of solid particles and the formation of the final structure28. Increasing GGBS substitution during alkali activation leads to the formation of larger quantities of C-(A)-S-H and N-A-S-H gels. As a result, porosity is reduced, a denser and more homogeneous microstructure develops, and both strength and elastic modulus increase29,30. A cement-based mixture that satisfies specific performance requirements can be produced by adjusting the proportions of available raw materials through experimental design optimization. In conventional mixture design, both prescriptive and performance-based approaches can be used for optimization31. Recently, Response Surface Methodology (RSM) has been widely applied for developing mortar and concrete mix proportions32–34. In FA/GGBS geopolymer systems, important variables include the concentration of the alkali activator and the ratio of FA to GGBS35. The type, amount, and volume fraction of fibers, along with the binder composition, curing environment, and curing age, significantly influence the strength characteristics of fiber-reinforced geopolymer composites36. Another key factor influencing mechanical performance is the interaction between fibers and the geopolymer binder. A strong interfacial transition zone (ITZ) between the fiber and the geopolymer matrix enhances the load-bearing capacity of the composite37. Most alkaline solutions employed in the polymerization process consist of sodium hydroxide or potassium silicate and form gel-phase mixtures that may contain lingering insoluble particles, resulting in lower compressive strength25,38. The central composite design (CCD) method is commonly used for optimizing mixture proportions in cement-based materials. In CCD, experimental points are distributed around a central point in a star-shaped configuration within a two-level factorial design. This method is highly efficient because it allows simultaneous optimization of multiple parameters and can accommodate up to six variables13,23,39. The primary objectives of this study are: (1) to develop a CCD-based RSM model for predicting and optimizing the mechanical performance of alkali-activated mortars incorporating NS, NA, and PPF; (2) to assess the durability of the optimized mixtures under sulfuric acid, sodium chloride, and magnesium sulfate exposure; (3) to evaluate the CO₂ emission profile of the AAM system in comparison with conventional OPC concrete; and (4) to characterize the microstructural mechanisms using SEM analysis. The use of industrial by-products (FA and GGBS) as primary binders reduces both material cost and carbon footprint, thereby contributing to sustainable construction strategies. Experimental work Materials Seventeen distinct alkalis-activated mortar formulations were developed, incorporating varying quantities of PPF, NS, and NA. The dosage levels were 0%, 0.5%, and 1% for PPF, and 0%, 1%, and 2% for both NA and NS by mass of binder13,23. The binder system consisted of GGBS and low-calcium FA, both conforming to the specifications of ASTM C618. The chemical compositions of FA and GGBS are presented in Table 1. The aim of this study was to investigate the effect of nanomaterials (NS and NA) and PPF on both compressive and flexural strength. Natural unprocessed sand was used as fine aggregate, and its grading was evaluated through sieve analysis in accordance with ASTM standards. The total binder content was fixed at 700 kg/m³ (350 kg FA + 350 kg GGBS for the control mix), and the binder-to-alkaline solution mass ratio was maintained at 0.5 for all mixtures. The sodium hydroxide to sodium silicate mass ratio was kept constant at 1:2.5 for all batches. Table 1Chemical composition of FA and GGBS13,23.ComponentCaOSiO2Al2O3Fe2O3MgOTiO2SO3K2OP2O3Mn2O3Na2OSrOLOI(FA%)15.4848.4317.1511.961.352.680.820.410.40.170.00190.21.47(GGBS%)47.7528.178.60.423.890.941.450.290.060.470.020.0760.2 Chemical composition of FA and GGBS13,23. The alkali activators used in this study were sodium hydroxide (NaOH) and sodium silicate (Na₂SiO₃). The sodium silicate solution, procured from a local supplier, contained Na₂O (13.7%), SiO₂ (29.4%), and water (55.9%) by mass. Sodium hydroxide with 98% purity and a flaky form was used, and a molarity of 12 M was adopted as it demonstrated optimal performance in previous studies40–43. In a recent research study, polypropylene fibers with a length of 6 mm were incorporated at dosage levels of 0.5% and 1%44. The main properties of the nanomaterials and polypropylene fibers used in this study are summarized in Table 2. The particle sizes of nano-silica and nano-alumina range from 20 to 30 nm, exhibiting amorphous and gamma forms. The chemical compositions from China include nano-alumina with a purity of 99.8% for Al2O3 and 99.9% for SiO2 in nano-silica. Table 2Properties of nanomaterials and PPF13.AdditivesParticle sizePurityPhaseColor(NS)Nano-Silica20–30 nm99.8%AmorphousWhite(NA)Nano-Alumina20–30 nm99.9%GammaWhite(PPF)- Polypropylene Fiber6 mm--Grey/White Properties of nanomaterials and PPF13. The physical and mineralogical characteristics of the materials used in this study are illustrated in Fig. 1. The grading distribution of the natural fine aggregate obtained from sieve analysis is presented in Fig. 1(a). The results indicate that the sand falls within the acceptable grading limits for mortar production according to ASTM standards. Figure 1(b) illustrates the X-ray diffraction (XRD) patterns of GGBS and FA. The FA pattern is characterized by several high-intensity peaks, particularly within the range of 10°–50°, indicating the presence of crystalline phases. The primary crystalline phases identified in FA include quartz (SiO₂), mullite (3Al₂O₃·2SiO₂), and hematite (Fe₂O₃). Sharp peaks around 20°–30° specifically indicate the presence of quartz. A slightly elevated baseline beneath these peaks suggests that FA also contains an amorphous (glassy) phase. This amorphous phase, mainly composed of silica and alumina, plays a crucial role in alkaline activation because it dissolves and contributes to the formation of binding gel phases. In contrast, the absence of sharp and well-defined peaks in the GGBS pattern indicates that the slag is predominantly amorphous. Such amorphous structures are typical of materials that have cooled rapidly without crystallization. The amorphous phase in GGBS contains reactive components such as calcium, silica, and aluminum. A broad and diffuse hump is observed between 20° and 35°, which is characteristic of a glassy structure. These amorphous materials readily dissolve under alkaline activation, forming binder phases such as C-A-S-H and N-A-S-H gels, which enhance mechanical performance. Although both materials are suitable for alkaline activation, the combination of FA and GGBS provides synergistic effects due to the faster reaction kinetics of GGBS. Properties of aggregates and binders. a Sieve analysis of natural fine aggregate23, b XRD pattern of GGBS and FA. Mix proportion and method of mix design This research study employed CCD within RSM framework to optimize the mix proportion of alkali-activated mortar. CCD is a well-established experimental design consisting of three components: (1) a two-level factorial design (corner points at coded levels ± 1), (2) axial (star) points at coded levels ± α, and (3) replicated center points45. For three factors at three levels, a face-centered CCD (α = 1) was selected, yielding 17 experimental runs: 8 factorial points, 6 axial points, and 3 center-point replicates. This design enables estimation of a full second-order polynomial response surface, capturing main effects, quadratic effects, and two-factor interaction effects. Design-Expert software was used for experimental design generation, model fitting, and optimization46–48. A comparison between predicted and actual responses indicated that the quadratic model could effectively predict the performance of these nano-enhanced mortar mixes, as summarized in Table 3. Three independent variables were considered: nano-silica content (A: NS, 0–2% by mass of binder), nano-alumina content (B: NA. 0–2% by mass of binder), and polypropylene fiber content (C: PPF 0–1% by volume of binder). The coded levels are defined as −1 = lower bound, 0 = center point, and + 1 = upper bound. The relationship between coded (Xi) and actual values is: Xi = (Actual – Center)/(Range/2). For NS and NA, the coded levels correspond to − 1 = 0%, 0 = 1%, and + 1 = 2%. For PPF, the coded levels correspond to − 1 = 0%, 0 = 0.5%, and + 1 = 1%. The variables and their corresponding ranges are presented in Table 3. Table 3Variables and percentages of variable ranges.VariablesSymbolLevel of VariablesRemarks−101Nano-silicaAa0.0%1.0%2.0%By mass of FA+GGBS binderNano-aluminaBa0.0%1.0%2.0%By mass of FA+GGBS binderPolypropylene fiberCc0.0%0.5%1.0%By volume of binderaRoughness of material addition in the binderbRoughness of material addition in the bindercRoughness of fiber addition Variables and percentages of variable ranges. aRoughness of material addition in the binder bRoughness of material addition in the binder cRoughness of fiber addition The RSM quadratic model used to relate the response Y to the coded independent variables is given by Eq. 1: Where Y is the predicted response (e.g., compressive strength, MPa); is the intercept; are linear coefficient; are quadratic (curvature) coefficients; are interaction coefficient; Xi and Xj are coded independent variables; and is the residual experimental error. The model was fitted using least squares regression, and its adequacy was evaluated using analysis of variance (ANOVA), the coefficient of determination (R2), adjusted R2, and predicted R2. The lack of fit test was used to verify that no significant systematic model error existed. Each mixture contained a total binder content of 700 kg/m³. The control mix consisted of 350 kg/m³ FA and 350 kg/m³ GGBS. When nanomaterials were added as a percentage of binder mass, the FA and GGBS contents were proportionally reduced to maintain the total binder content as close as possible to 700 kg/m³ (approximately 343–350 kg/m³ each depending on additive dosage). This minor variation arises from the RSM additive-inclusion method and does not represent an intentional change in the FA: GGBS ratio, which was maintained at 1:1 throughout the study. The binder-to-alkaline solution ratio was fixed at 0.5, while the NaOH-to-Na₂SiO₃ ratio was maintained at 1:2.5. Natural sand was used as the fine aggregate49, and a superplasticizer (Glenium 51) was incorporated to regulate workability. The detailed mix proportions of all experimental runs are presented in Table 4. Table 4Experimental mix design of geopolymer mortar.Mix No.RunNSNAPPFCFC SubdivisionFAKg/m3GGBSKg/m3S.Hkg/m3S.Skg/m3F.Aggkg/m3SP%M11−11−1Factorial Points346.5346.51002501033.4853M22−111346.5346.51002501033.4853M34−1−113503501002501033.4853M4711−13433431002501033.4853M581113433431002501033.4853M6121−1−1346.5346.51002501033.4853M714−1−1−13503501002501033.4853M8171−11346.5346.51002501033.4853M9300−1Axial Points346.5346.51002501033.4853M105010344.75344.751002501033.4853M116001346.5346.51002501033.4853M1290−10348.25348.251002501033.4853M1311−100348.25348.251002501033.4853M1416100344.75344.751002501033.4853M1510000Center Points3463461002501033.4853M16130003463461002501033.4853M17150003463461002501033.4853The numerical numbers such as (−1,0,1) has been defined by design expert software and each of numerical number defined for percentages of (For NS and NA: −1 = 0%, 0 = 1%, and 1 = 2%) and (For PPF: −1 = 0%, 0 = 0.5%, and 1 = 2%). Experimental mix design of geopolymer mortar. The numerical numbers such as (−1,0,1) has been defined by design expert software and each of numerical number defined for percentages of (For NS and NA: −1 = 0%, 0 = 1%, and 1 = 2%) and (For PPF: −1 = 0%, 0 = 0.5%, and 1 = 2%). The overall experimental procedure consisted of four key steps: designing the experimental trials, conducting experiments and collecting data, establishing a numerical model using RSM, and optimizing and validating the developed model49. The CCD approach is one of the most widely used experimental designs within RSM due to its efficiency in evaluating the effects of multiple variables45. As illustrated in Fig. 2, the design includes factorial points located at the corners of the cube (± 1 levels), axial or star points positioned along each axis, and center points representing the midpoint of the experimental domain48. Central composite design (CCD). For several issues, cement-based materials have been subjected to RSM’s experimental improvement50. The objective of this method is to enhance mixture design, considering various variables such as the development of mechanical strength. This is achieved through iterative experimentation, accounting for factors like nano-alumina and nano-silica percentages, polypropylene fiber, alkali-activated mortar, liquid preparation solution conditions, and curing environment. Equation (2) is the regression model used in RSM in addition to CCD. The relationship between the response Y and the experimental factors {Xi} was described using an RSM regression model. The coefficient β quantifies the contribution of each factor and represents experimental random error. This model enables prediction of Y within the studied domain and support statical evaluation and optimization. A generalized regression form used in RSM is presented in Eq. 2. where k denotes how many variables have been optimized; After the regression coefficients, Y is the response variable; Xi stands for the independent variables and the random error of the estimated answer. The following is an example of a second-order regression model that can be produced if the regional tests show that there is a curvature: A second order polynomial model was adopted in the RSM framework to relate the response y to the coded factors Xi, The quadratic term quantify the main effects, curvature, and combined effects of the variables, enabling response prediction and optimization within the experimental domain. Mixing, casting and curing Sodium silicate was combined with NaOH flakes after the NaOH had been dissolved in distilled water and allowed to stand for 4 h to reach the required concentration. The prepared alkaline solution was then stored for 24 h before use. The mixing procedure was carried out as follows: (1) dry material (FA, GGBS, nanomaterials, and fine aggregate) were blended in a mechanical mixer for 2.5 min; (2) the alkaline solution with superplasticizer was gradually added and mixed for an additional 2 min; (3) for fiber containing mixtures, PPF was introduced slowly during continued mixing for a further 2 min to ensure that uniform fiber distribution. All mix proportions are expressed per 1 m3. Cubic specimens (50 × 50 × 50) and prism (40 × 40 × 160) mm were filled with AAM and then repeatedly vibrated in the vibration table for 30 s per layer until surface leveling23,40. Following casting, all specimens were sealed with plastic sheets to prevent moisture loss during the initial setting period (24 h). Subsequently, specimens were cured under ambient laboratory condition at 23 ± 2 ℃ until the testing age of 28 days, in accordance with ASTM C10951 until the date of the hardened test52. Compressive strength specimens were used for each mixture49, and flexural strength was assessed using the ASTM C348 standard53. Three replicate specimens per mixture were used for each mechanical test. For the durability assessment, specimens were immersed in three chemical solutions after 28 days of ambient curing: (1) 5% by the weight of each chemical compound with water to produce the exposure solution for sulfuric acid (H2SO4), (2) 5% sodium chloride (NaCl) solution with pH = 7; and (3) 5% magnesium sulphate (MgSO4) solution with pH = 6.8. All specimens were immersed for 90 days at room temperature. Residual compressive strength was measured at the end of the exposure period and compared with reference specimens cured in water. Result and discussion RSM model fitting and statical analysis The RSM quadratic model was fitted to the experimental data for two responses: 28-day compressive strength (CS) and 28-day flexural strength (FS). The model adequacy was assessed using ANOVA, and the results are presented in Tables 5 and 6 for compressive strength and flexural strength, respectively. The F-value confirms that both models are statistically significant (P < 0.0001). The lack of fit F-values is not significant (P > 0.05), indicating that the quadratic model adequately represents the experimental data within the studied domain. Table 5ANOVA table for RSM quadratic model for 28-day compressive strength.SourceSum of SquaresDfMean SquareF-ValueP-ValueRemarksModel1524.389169.3748.56< 0.0001SignificantA: NS120.451120.4534.530.0004B: NA390.211390.21111.93< 0.0001C: PPF45.67145.6713.090.0067AB28.90128.908.290.0197AC12.34112.343.540.0962BC18.78118.765.380.0471A289.43189.4325.650.0009B2201.561201.5657.82< 0.0001C238.12138.1210.940.0103Residual24.3773.48--Lack of Fit16.2453.250.800.6134Not significantPure Error8.1324.07--Cor Total1548.716--- ANOVA table for RSM quadratic model for 28-day compressive strength. Table 6ANOVA table for RSM quadratic model for 28-day flexural strength.SourceSum of SquaresDfMean SquareF-ValueP-ValueRemarksModel24.1892.6932.47< 0.0001SignificantA: NS3.8413.8446.360.0002B: NA1.2111.2114.610.0064C: PPF8.7618.76105.78< 0.0001AB0.4210.425.070.0585AC2.3112.3127.890.0011BC0.8910.8910.750.0135A21.5611.5618.840.0033B23.1213.1237.680.0005C20.6710.678.090.0247Residual0.5870.083--Lack of Fit0.3850.0760.760.6412Not significantPure Error0.220.1--Cor Total24.7616--- ANOVA table for RSM quadratic model for 28-day flexural strength. The Model F-value of 48.56 (P < 0.0001) confirm model significance. Individual term B (NA content) and B2 have the largest F-value (111.93 and 57.82), respectively, indicating that nano-alumina content and its quadratic effect are the dominant factors influencing compressive strength. The R2 = 0.964, adjusted R2 = 0.963, and predicted R2 = 0.921 are in close agreement (difference < 0.2), containing the good predictive capability of the model. The adequate precision that ratio of 22.4 (> 4) further confirm that the model signal to noise ratio is acceptable for navigating the design space. For the flexural strength, the model F-Value pf 32.47 (P < 0.0001) confirm significance. PPF content (C) has the highest F-value (105.78), indicating it is the most influential factor for flexural strength, consistent with the crack-bridging mechanism of polypropylene fiber. R2 = 0.977, adjusted R2 = 964, and the predicted R2 = 0.905 confirm the adequacy of this model as well. The regression equations for compressive strength (CS, MPa) and flexural strength (FS, MPa) in terms of coded variables (A = NS, B = NA, C = PPF) are given by Eq. 3 and Eq. 4: In Eq. (3), the positive coefficient of B (NA) and A (NS) confirm that increasing nano-alumina and nano-silica content enhances compressive strength, with NA exerting the greater effect. The negative quadratic terms (A2, B2, C2) indicate that response surface exhibits downward curvature, implying the existence of an optimum dosage beyond which strength diminishes. The negative coefficient of C (PPF) for compressive strength reflects the known slight dilution effect of fiber addition on matrix density. In the Eq. (4), C (PPF) has the largest positive linear coefficient, confirming it dominant role in flexural performance through crack bridging. Compressive strength An examination of the alkali-activated mortar’s compressive and flexural strengths is shown in Fig. 3. The figure illustrates the impact of nanomaterials and varying percentages of PPF on the material. The compressive strength of alkali-activated mortar, a critical characteristic for designing specific structures, is similarly crucial for alkali-activated binders. Compressive strength in alkali-activated systems is highly dependent on the concentration of the alkaline solution. Effect of nano-silica, nano-alumina, and polypropylene fiber on compressive strength of AAM. Figure 3(a) and (b) compare the compressive strength of two nanomaterials in alkali-activated mortar. For a mixture with 2% nano-alumina (M1), after 28 days, the material’s compressive strength reached its maximum of 82 MPa. Conversely, the application of 2% nano-silica (M6) significantly increased the compressive strength of AAM, reaching about 72 MPa after 28 days. The results were substantially impacted when compared to when both nanomaterials (M4) were used together at a rate of 2%, yielding a compressive strength of about 65 MPa (M1, M6). Furthermore, samples with 1% of both nanomaterials increased AAM’s compressive strength and outperformed (M6). Figure 3(c) and (d) illustrates the comparison of compressive strength results of AAM between PPF and NS. The compressive strength of the sample (M3) containing 1% PPF is 67 MPa. However, when 2% NS is added (M8), the compressive strength decreases to 64 MPa. This indicates that the combination of 2% nano-silica with 1% PPF has an insignificant impact on the compressive strength of AAM compared to samples containing only 2% NS, which exhibit a higher effect on compressive strength compared to M3 and M8. On the other hand, the sample containing 1% NS with 0.5% PPF shows a slight decrease in compressive strength compared to control samples (M7), (M3), and (M8), measuring about 63 MPa. Figure 3(e) and (f) examines the compressive strength results of PPF and nano-alumina in AAM. The sample’s compressive strength containing 1% PPF (M3) is 67 MPa. However, adding 2% NA (M2) increases the compressive strength to 71 MPa. This indicates that 2% nano-alumina with 1% PPF significantly enhances the compressive strength of AAM compared to samples containing only 2% nano-silica with 1% PPF (M8), which experiences a decrease and loss of strength performance compared to (M3). In contrast to M3 and M2, the sample with 2% NA obtains a higher compressive strength of AAM. In contrast to control samples (M7), (M3), and (M2), the sample containing 1% NA with % PPF exhibits an improvement in compressive strength to 74 MPa. However, it is still less than that of (M1), which measures 82 MPa. In every aspect, nano-alumina exhibits superior performance compared to nano-silica, and combining 2% of both yields enhanced compressive strength. Figure 3(g) shows a strong match between the model’s predictions and the actual compressive strength of concrete after 28 days. Most of the points fall close to the diagonal line, which suggests the model is making very accurate predictions. The high R² value confirms that the model does a good job capturing how different mix designs affect strength. This kind of comparison is commonly used in research to check how reliable a concrete strength prediction model is54,55. To check whether the model meets the requirements of regression analysis, a normal probability plot of studentized residuals was created showed on Fig. 3(h). The residuals show a nearly straight-line pattern along the reference line, with only small deviations at the ends. This confirms that the residuals are normally distributed, which is an important requirement for valid regression analysis56,57. Studentized residuals are better than ordinary residuals because they adjust for differences in variance, making the model assessment more reliable58. The residual plot does not show any clear patterns or trends, which indicates that the model does not have significant errors or missing relationships. This confirms that the model is suitable for predicting concrete compressive strength59. This section presents typical residual mechanical strength data plots to evaluate compressive and flexural strength and validate the model’s applicability. The residuals obtained from the ANOVA results play a crucial role in assessing the adequacy of the model. The fact that a straight line can be formed on a plot showing the link between the studentized residuals and the average probability percentage provides more evidence for the correctness of the model. Flexural strength Alkali-activated binders share the same flexural strength as alkali-activated mortar, which is an essential property for building certain structures. The flexural strength in alkali activation is significantly influenced by the alkaline solution’s concentration. Figure 4 compares the flexural strength findings of two nanomaterials with PPF in alkali-activated mortar. At 28 days, the mixture attains its highest flexural strength of 12 MPa, identified as M12, and is composed of % PPF and 1% nano-silica. When 2% nano-silica and 1% PPF were used, alkali-activated mortar’s flexural strength significantly improved and increased (M8), reaching roughly 11 MPa after 28 days. In contrast to (M1, M6, M9, and M4), which incorporate nanomaterials without PPF, the combined use of 1% for both nanomaterials and 0.5% PPF (M16) resulted in enhanced flexural strength outcomes. Polypropylene fiber potentially has a positive effect on AAM’s flexural strength and ductility. Additionally, samples containing nanomaterials with polypropylene fiber exhibited superior performance compared to samples without PPF. Flexural strength of AAM as affected by nano-sized particles of silica, alumina, and polypropylene fibers. Figure 4(a) and 4(b) compare the flexural strength test results conducted on AAM using nano-alumina and nano-silica, respectively. The sample containing 2% NA (M1) has a flexural strength of 9 MPa. Adding 2% of NS (M4) increases the flexural strength by 10 MPa. It shows that 2% of nano-alumina with 2% of nano-silica have a significant performance on the flexural strength of AAM compared to samples containing only 2% of NS and NA (M6 and M1). However, sample M9, which has 1% of NA and 1% of NS, only marginally improved the compressive strength of AAM over M1 in comparison (M6 and M4). Figure 4(c) and (d) compare the AAM flexural strength data for nano-silica and polypropylene fiber, respectively. The flexural strength of the sample containing 1% PPF (M3) is 9.3 MPa. Adding 2% of NS (M8) increases the flexural strength by 11.1 MPa. It shows that 2% of nano-silica has an insignificant effect on the flexural strength of AAM compared to samples without NS. On the other hand, the sample contains 1% NS along with % PPF, and the flexural strength is dramatically rises compared to other mixes comprising nanomaterials and PPF, and it has the maximum flexural strength. Figure 4(e) and (f) compare AAM flexural strength results between polypropylene fiber and NA. The flexural strength of the sample contains 1% PPF (M3) is 9.3 MPa. By adding 2% of NA (M2), the flexural strength increases by 10.6 MPa. It shows that 2% of nano-alumina has an insignificant effect on the flexural strength of AAM compared to samples without NA. However, the sample containing 1% NA and 0.5% PPF (M13) shows a slight decline in flexural strength to 9.2 MPa. Indeed, including polypropylene fiber improves performance compared to samples lacking polypropylene fiber. However, incorporating 2% of both nano-alumina with % PPF and nano-silica with % PPF leads to an even more significant enhancement in flexural strength. Moreover, utilizing both 2% nanomaterials with 1% PPF significantly boosts flexural strength. The compressive and flexural strengths were evaluated at 28 days post-curingdemonstrates that the plot displays the relationship between compressive strength at 28 days, ranging from 55 to 85 MPa, flexural strength at 28 days, ranging from 8 to 12 MPa, and the design space type, with data points colored according to experimental run (Fig. 5). The correlation coefficient of −0.322 indicates a weak negative relationship between the plotted variables, suggesting that the relationship between these mechanical properties is influenced by multiple factors rather than a simple linear trend60. This type of three-dimensional representation is particularly useful for visualizing how multiple response variables interact across the experimental design space61. The compressive and flexural strengths were evaluated at 28 days post-curing. Multi objective optimization Multi-objective optimization was performed using the RSM desirability function approach, targeting the simultaneous maximization of both compressive and flexural strength. The optimization criteria were set as NS in range (0–2%); NA target = 0 (unconstrained in optimization); PPF target = 0 (unconstrained); maximize compressive strength (range: 55.4–82 MPa, importance = 3); maximize flexural strength (range: 7.98–12.98 MPa, importance = 3). The optimal solution identified by the CCD-RSM model corresponded to NS = 0% (coded − 1), NA = 1% (coded 0), and PPF = 0.5% (coded 0), with a predicted compressive strength of 71.96 MPa, flexural strength of 9.04 MPa, and an overall desirability of 0.638. This optimal mix represents the best compromise between strength and durability performance across the studied domain. Chemical attacks of AAM Sulfuric acid Figure 6. The Response plot and Prediction of Compressive Strength of AAM exposed under Sulfuric Acid solution presents the response surface plots, contour plots, and predicted versus actual results illustrating the influence of NS, NA, and PPF on the compressive strength of AAM exposed to sulfuric acid solution. In Fig. 6. The Response plot and Prediction of Compressive Strength of AAM exposed under Sulfuric Acid solution, the scatter diagram depicts the ordinate’s expected value and the abscissa’s actual value. Each point closely aligns with the straight-line y = x, demonstrating a high level of model fitting. This indicates that the calculated predicted values closely match the actual values determined by the test. The effects of adding different percentages of NS, NA, and PPF as additives on the 90-day compressive strength of AAM in sulfuric acid solution are displayed in Fig. 6. The Response plot and Prediction of Compressive Strength of AAM exposed under Sulfuric Acid solution. Adding nanomaterials to the mixture causes the compressive strength to rise roughly linearly with increased content. The predicted and actual plots for both 28-day compressive strength and compressive strength after sulfuric acid exposure show that most data points lie close to the diagonal line. This indicates a good agreement between the experimental results and the predicted values obtained from the CCD-RSM model, confirming the reliability of the developed model. Regarding the durability results, the compressive strength after sulfuric acid exposure shows a reduction compared with the normal condition. This reduction occurs because sulfuric acid reacts with the geopolymer matrix, which can lead to partial decomposition of binding gels and microstructural damage. The acidic environment may dissolve some reaction products and weaken the bond between particles, resulting in a loss of mass and a reduction in strength. This suggests that the primary factors influencing the compressive strength of the mortar are NA, NS, and PPF. This is a result of the high aluminosilicate concentration of the FA and GGBS, which act as binders. This causes the mixture’s Ca content to rise, which causes further C-(A)-S-H to be produced under the effect of an alkali activator and coexist with N-A-S-H gel. After 90 days of immersion in a 5% H2SO4 solution (pH = 1.2), the residual compressive strength of all mixtures was measured. The CCD-RSM model for post-acid compressive strength showed good agreement with experimental data, with data points closely aligned along the predicted vs. actual diagonal Fig. 6. The Response plot and Prediction of Compressive Strength of AAM exposed under Sulfuric Acid solution, confirming model reliability for durability prediction. The residual strength ranged from approximately 25.6 MPa (low NA/NS, no PPF) to 58.6 MPa (2% NA + 2%NS + 0.5% PPF), representing a retention of 44–71% of the 28-day control strength. The strong linear relationship demonstrated that the developed model accurately predicts the residual compressive strength of mortar specimens exposed to sulfuric acid across a wide range of values (25–60 MPa). This visualization confirms the model’s reliability for predicting concrete durability under acidic conditions. The Response plot and Prediction of Compressive Strength of AAM exposed under Sulfuric Acid solution. Sodium chloride After 90 days of immersion in a 5% NaCl solution, the residual compressive strength ranged from approximately 39.7 MPa to 78.7 MPa across all mixture Fig. 7. The NaCl solution had a near neutral pH = 7, resulting in less severe chemical attack compared to the acidic environment. The RSM model for NaCl exposure achieved R2 = 0.97, confirming good predictive accuracy. Nanomaterial content (NA and NS) was the primary driver of chloride resistance, with the minimum strength of 39.67 MPa and maximum of 78.69 MPa corresponding to the lowest and highest nanomaterial dosages, respectively. PPF addition caused a minor reduction in compressive strength compared to fiber-free mixes, though it significantly improved crack resistance and ion permeation resistance by reducing microcrack connectivity. The Response plot and Prediction of Compressive Strength of AAM under Sodium Chloride. Polypropylene fiber, nano-alumina, and nano-silica: their effects added as additives with different proportions of NS, NA, and PPF on the AAM’s 28-day compressive strength under Sodium Chloride solution are shown in Fig. 7(a, b, c, d, e, and f). The incorporation of nanomaterials into the mixture leads to a nearly linear increase in compressive strength as the content of nanomaterials increases. On the steeply curved surface, the minimum strength falls to 39.67 MPa, and the maximum strength rises to 78.69 MPa with respect to NS and NA. When PPF is added to the mixtures, the strength of compression decreases compared to the mixes without PPF, although the change is minimal. PPF exhibits extraordinary advantages in the chemical resistance of AAM and plays an essential role in fostering a good bond between binders and aggregates. These results demonstrate that the main determinants of the mortar’s compressive strength are NA, NS, and PPF. This is attributed to using FA and GGBS as binders, which have a chemical composition rich in aluminosilicate content. Because of the alkali activator’s influence, the mixture’s Ca concentration rises, causing more C-(A)-S-H to be produced in addition to the N-A-S-H gel. Magnesium sulfate After 90 days of immersion in a 5% MgSO4 solution, residual compressive strength ranged from approximately 47.3 MPa to 82.7 MPa. The relatively higher residual strengths under MgSO4 compared to H2SO4 exposure are consistent with the milder pH of the sulfate solution, nearly 6.8, and the known resistance of geopolymer matrices to sulfate attack, which is attributed to the absence of calcium hydroxide (portlandite), a primary target for ettringite formation in the OPC system. The RSM model for MgSO4 exposure achieved R2 = 0.962. Some scatter was observed at high strength values (65–80 MPa), which may reflect the complex interaction between Mg2+ and the aluminosilicate gel phase at higher gel densities62. In Fig. 8 (a, b, c, d, e, f), the influence of the interaction between nano-silica, nano-alumina, and polypropylene fiber added as additives with varying percentages of NS, NA, and PPF on AAM’s 28-day compressive strength under Magnesium sulfate Solution is presented. The number of nanomaterials added to the mixture causes the compressive strength to rise almost linearly as their content increases. The maximum strength increases to 82.74 MPa with respect to NS and NA, whereas the minimum strength increases to 47.34 MPa on the steeply curved surface. Upon adding PPF to the mixtures, the compressive strength decreases compared to the mixes without PPF, though the change is minimal. PPF exhibits extraordinary advantages in the chemical resistance of AAM and plays an essential role in fostering a good bond between binders and aggregates. The Response plot and Prediction of Compressive Strength of AAM exposed under magnesium sulfate. These results highlight that the main variables affecting the mortar’s compressive strength are NA, NS, and PPF. This is attributed to using FA and GGBS as binders, which have a chemical composition rich in aluminosilicate content. As a result, the mixture’s Ca concentration rises, which causes more C-(A)-S-H to be produced and to coexist with N-A-S-H gel when an alkali activator is applied. Optimization results for AAM The CCD-RSM multi-objective optimization procedure was applied to simultaneously maximize compressive strength, flexural strength, and durability performance. Using the desirability function, the global desirability of the optimal solution (NS = 0%, NA = 1%, PPF = 0.5%) was calculated as D = 0.638. The optimized predicted compressive strength of 71.96 MPa and flexural strength of 9.04 MPa represent a well-balanced high-performance mix, validated by the close agreement between predicted and experimental values (within ± 3% for compressive strength and ± 5% for flexural strength across the 17 runs). This solution also corresponded to acceptable durability performance, with residual strengths of approximately 52 MPa (H2SO4) and 65 MPa (MgSO4) after 90-day exposure. Obtaining the optimal value for every response in a single domain is challenging. Therefore, a multi-objective optimization approach is proposed as the most effective method for achieving an ideal solution that satisfies the requirements of all responses. After creating and validating ANOVA models for each response, the best practical answers were identified by utilizing a multi-objective optimization technique63. The core aim of the optimization study was to ascertain suitable values for the independent variables to fulfill the optimization objectives. Employing RSM technique proved effective in enhancing two responses influenced by three variables: NS, NA, and PPF. The CCD with the RSM approach yielded the following optimal settings listed in Table 7. According to Fig. 6, the optimum desirability solution for tests 1 through 17 was 0.638. Table 7Optimization standards of individual responses for AAM.A: NSIs in range−113B: NAIs target = 0−113C: PPFIs target = 0−113Strength under compression 28 days, in order to achieve the optimization goals, the primary purpose of the study that was conducted on optimization was to determine the appropriate values for the independent variables.Maximize55.4823Flexural strength 28 daysMaximize7.9811.953 Optimization standards of individual responses for AAM. Examining the compressive strength at 28 days in Fig. 6, the predictive finding for mixtures containing nano-alumina and polypropylene fiber is 66.75 MPa. This implies that the mixture corresponding to this MPa value is indicated on the chart, revealing the optimum percentages of nano-alumina at 1.5% of binders and PPF at approximately 0.25%. Furthermore, the feasibility changes for mixtures incorporating percentages of PPF and nano-silica. The predictive results for these mixture contents indicate that nano-silica at approximately 1.5% and PPF at about 0.7% yield better results than the percentages in the mix design. The graph depicting the optimal response is presented in Fig. 9. The results from the multi-objective optimization reveal that the optimal levels are − 1 for NS, 0% for NS, 1% for NA, 0% for NA, and 0% and 0.5% for PPF. The corresponding optimal compressive and flexural strength values at 28 days are 71.96 MPa and 9.035 MPa, respectively. In this investigation, the significance of the responses (compressive and flexural strength) was determined to be equal, aligning with the overarching objective of the study. The desirability of the optimal solutions was calculated to be 0.637. The optimal mix obtained from the desirability analysis does not necessarily correspond to the maximum compressive or flexural strength values. This is because the optimization process considered multiple responses simultaneously, including compressive strength, flexural strength, and durability performance. Although the highest compressive strength 82 MPa, and flexural strength, 12 MPa were observed in specific mixes, this mixture did not provide the best overall performance when other parameters were considered. In the desirability analysis, equal importance was assigned to all responses, and the optimized solution represents the best compromise between strength and durability characteristics. The numerical optimization contour with desirability of 1 and the solution 1 out of 17. CO2 emission The environmental sustainability of the optimized AAM mixture evaluated through a cradle to gate CO2 emission analysis, using material specific emission factors sourced from published literature. The CO2 emission for each mixture component was calculated using Eq. 5: The emission factor adopted in this study are: fly ash = 0.027 kg CO2/kg64,65; GGBS = 0.15 kg CO2/kg66–68; and sodium silicate = 0.45 kg CO2/kg69; sodium hydroxide = 1.95 kg CO2/kg70,71; nano-silica 0.00084 kg CO2/kg72–74; nano-alumina = 0.003 kg CO2/kg75,76; and fine aggregate = 0.013 kg CO2/kg77. These factors represent the energy and process emission associated with the material production, that including mining, processing, and transport to the construction site. The sustainability assessment of the alkali-activated combination was based on the CO2 emissions connected with its manufacturing materials78,79. Valente et al. provided CO2 emission factors for fly ash, GGBS, sodium silicate, and sodium hydroxide56, while the emission data for other materials are presented in Table 8. Table 8Equivalent CO2 emission for each material contributed to the mixture.MaterialsContent (kg/m3)Emission Factor (kg CO2/kg)CO2 Emission (kg CO2/m3)RolesJustificationFly Ash3500.0279.45Replace cement, significantly lowering CO2 emission.Fly ash is a coal combustion by product with minimal processing emission. The emission factor account for collection, processing, and transportation. Studies show 50–70% reduction in embodied carbon when replacing cement64,65.GGBS3500.1552.5Replaces cement and conserves natural resources and energyGGBS is a steel industry by product the emission factor includes grinding and transportation avoids clinker production emission66–68.Nano Silica2% by wt0.00080.021Improve strength and durability.The emission factor reflects the energy intensive production process involving precipitation or flame synthesis. Despite its higher specific emission, the small dosage (2% by wt of binder)73,74Nano Alumina2% by wt0.0030.0056Enhance mechanical performance and durabilityProduction involves energy intensive calcination and milling processes. The emission factor is higher than conventional materials but is justified by the minimal quantity required and substantial performance improvements in mechanical strength and durability75,76Sodium Silicate1000.4545Activate fly ash, and slag contributing to moderate CO2 emissionProduced through high temperature fusion of sand and sodium carbonate or by dissolving silica in caustic soda70.Sodium Hydroxide2501.95487High CO2 emission activator but necessary for the geopolymer process.Manufactured through chlor-alkali electrolysis process which is highly energy-intensive. Despite high emission, it is essential for dissolving aluminosilicate materials and initiating geopolymerization reaction71.Fine Aggregate10330.01313.4Filler material reduces the amount of cement used and its consumption.Natural sand, the low emission factor reflects the natural availability and simple processing requirements compared to manufactured materials77. Equivalent CO2 emission for each material contributed to the mixture. The Total CO2 emission of the optimized AAM mixture is approximately 607.9 kg CO2/m3.Comprehensive LCA studies of FA-GGBS geopolymer concrete using SimaPro and MonteCarlo simulation have reported emission in the range of 203–253 kg CO2eq/m3, that reflect a 43% reduction compared to conventional concrete while confirming that chemical activators particularly NaOH and Na2SiO3 are the dominant carbon contributors80. The comparatively higher emission in the present study is primarily attributable to the elevated NaOH dosage (250 kg/m3 at 1.95 kg CO2/kg), which account for approximately 80% of total emission. Sodium hydroxide is the single largest contributor, accounting for approximately 487.5 CO2/m3 that 80% of total emissions, due to the energy intensive chlor-alkali electrolysis process used in its manufacture. In comparison to the OPC benchmark of around 819 kg CO2/m³, the 26% CO2 decrease seen in this experiment is in line with published literature ranges. While emphasizing that increasing alkali dosages might undermine or reverse this environmental benefit, comparative life cycle assessment (LCA) studies of alkali activated materials and OPC concrete have shown that geopolymer concrete produces significant CO2 savings when activator dosage is regulated81. According to research studies82,83, for comparison, ordinary Portland Cement concrete with a cement content of approximately 400 kg/m3 produces approximately 819 kg CO2/m3, based on a cement emission factor of approximately 0.93 kg CO2/kg. These observations collectively reinforce the finding that environmental competitiveness of FA/GGBS alkali activated system is critically contingent on the management of NaOH content and that meaningful further reduction in embodied carbon require either optimization of activator dosage or substitution with lower impact alkaline sources84. The optimized AAM mixture therefore represent a reduction of approximately 211 kg CO2/m3 compared to equivalent OPC concrete, corresponding to a CO2 savings of approximately 26%. This finding is consistent with the broader literature, which reports CO2 reduction of 20–40% for FA/GGBS based on geopolymer system relative to OPC concrete, depending on the activator type and dosage85. Davidovits (2015) reported a reduction of up to 55% in CO2 emissions from the Na2SiO3 solution. Consequently, the carbon factor for the Na2SiO3 solution can be calculated as 0.4569. The reported sodium hydroxide and fine aggregate emission factors were considered for geopolymer (GP) production86. The incorporation of fly ash and ground granulated blast-furnace slag contributes to reducing air pollution by mitigating the release of carbon dioxide (CO2) and carbon monoxide (CO) associated with cement production87. The alkali activator, In particular sodium hydroxide, represent the dominant emission hotspot, contributing nearly 80% of the total despite being at moderate dosages. This is primarily attributable to the energy intensive chlor-alkali electrolysis process used in NaOH manufacturing88. In contrast, fly ash and GGBS together contribute only around 62 kgCO2/m3, it is 10% of total, affirming the low emission penalty of utilizing industrial by product as binder precursors. These finding highlight that further reduction in the carbon footprint of alkali activated system are most effectively achieved by optimizing the NaOH dosage or substituting with alternative activator with lower embodied emissions. Scanning electron microscopy (SEM) analysis Figure 10 demonstrates the SEM microstructural analysis of alkali-activated mortar containing 0.5% PPF fiber combined with 1% and 2% NS and NA, which reveals significant changes in the microstructure affecting mechanical performance and durability. With a content of 0.5% PPF, the fibers are generally well dispersed throughout the matrix. This fiber helps control cracking by bridging microcracks and limiting their propagation. In addition, nanoscale fillers such as NS and NA enhance the fiber-matrix interfacial bond by improving contact and load transfer between the fibers and the surrounding matrix. At NS dosage of 1–2%, the particles are generally well dispersed, filling microvoids and refining the pore structure by reducing capillary pores. This contributes to faster early-age strength development, particularly at an NA content of 1%. However, increasing NA to 2% promotes particle agglomeration, similar to that observed with NS at higher contents. Moreover, the combined use of NS and NA may reduce matrix uniformity, potentially lowering overall homogeneity. Specimens that include 2% nano-alumina serve as effective fillers by occupying pore spaces and improving the interaction between the binder phase, which consists of FA and GGBS23,89. The main product of the polymerization reaction is N-A-S-H gel, which is formed when fly ash particles dissolve as a result of ambient curing. The densification of the entire matrix, which resulted in increased structural integrity, allows the fly ash alkali-activated mixes to display a more compact and dense microstructure90,91. The SEM analysis for the selected mix design. Conclusions This study demonstrated that reinforcing alkali-activated mortar (AAM) with nano-silica (NS), nano-alumina (NA), and polypropylene fire (PPF) effectively enhance both mechanical performance and chemical resistance. By utilizing industrial by-products, the study provides a sustainable alternative to traditional cement-based materials and supports the development of environmentally friendly construction solutions. The highest compressive strength of 82 MPa was obtained in mixtures containing 2% NA (0% NS, 0% PPF), while the maximum flexural strength of 12 MPa was achieved in the mixture with 1% NS and 0.5% PPF. ANOVA results confirmed that NA is the dominant factor influencing compressive strength, whereas PPF predominantly governs flexural strength. The highest compressive strength of 82 MPa was obtained in mixtures containing 2% NA (0% NS, 0% PPF), while the maximum flexural strength of 12 MPa was achieved in the mixture with 1% NS and 0.5% PPF. ANOVA results confirmed that NA is the dominant factor influencing compressive strength, whereas PPF predominantly governs flexural strength. ANOVA verified the statistical significance of the RSM quadratic models, with R² = 0.984 for compressive strength and R² = 0.977 for flexural strength, and a non-significant lack of fit (P > 0.05). The regression equations successfully quantified the individual and interaction effects of NS, NA, and PPF on mechanical performance. ANOVA verified the statistical significance of the RSM quadratic models, with R² = 0.984 for compressive strength and R² = 0.977 for flexural strength, and a non-significant lack of fit (P > 0.05). The regression equations successfully quantified the individual and interaction effects of NS, NA, and PPF on mechanical performance. Chemical durability tests showed that mixtures with higher NA and NS contents exhibited superior resistance to sulfuric acid, sodium chloride, and magnesium sulfate. The combination of 2% NS and 2% NA increased strength by more than 20% in sulfuric acid, while the inclusion of PPF improved chemical resistance by limiting microcrack development in aggressive environments. Chemical durability tests showed that mixtures with higher NA and NS contents exhibited superior resistance to sulfuric acid, sodium chloride, and magnesium sulfate. The combination of 2% NS and 2% NA increased strength by more than 20% in sulfuric acid, while the inclusion of PPF improved chemical resistance by limiting microcrack development in aggressive environments. SEM analyses revealed that the nanomaterials enhanced matrix density through microvoid filling, contributing to a more homogeneous structure and accelerating early-age strength gain. The formation of C-(A)-S-H and N-A-S-H gels with NS and NA further strengthened the microstructure. PPF improved the fiber–matrix interface, controlled crack propagation, and enhanced overall durability. SEM analyses revealed that the nanomaterials enhanced matrix density through microvoid filling, contributing to a more homogeneous structure and accelerating early-age strength gain. The formation of C-(A)-S-H and N-A-S-H gels with NS and NA further strengthened the microstructure. PPF improved the fiber–matrix interface, controlled crack propagation, and enhanced overall durability. Industrial by-products such as FA and GGBS played a significant role in reducing CO₂ emissions. The study confirmed that alkali-activated mortars exhibit a lower carbon footprint than conventional cement systems. Optimization helped improve cost and material efficiency by determining effective combinations of NS, NA, and PPF. Industrial by-products such as FA and GGBS played a significant role in reducing CO₂ emissions. The study confirmed that alkali-activated mortars exhibit a lower carbon footprint than conventional cement systems. Optimization helped improve cost and material efficiency by determining effective combinations of NS, NA, and PPF. The optimization conducted using Response Surface Methodology (RSM) and the central composite design (CCD) identified the mixture with 2% NA and 0.5% PPF as the most efficient in terms of mechanical and chemical performance. After multi-parameter optimization, the maximum compressive strength reached 82 MPa and the flexural strength reached 12 MPa at 28 days of curing. The optimization conducted using Response Surface Methodology (RSM) and the central composite design (CCD) identified the mixture with 2% NA and 0.5% PPF as the most efficient in terms of mechanical and chemical performance. After multi-parameter optimization, the maximum compressive strength reached 82 MPa and the flexural strength reached 12 MPa at 28 days of curing. Overall, the results demonstrate that alkali-activated mortars reinforced with NA, NS, and PPF offer a promising pathway for developing high-performance, durable, and environmentally sustainable building materials. These materials support low-carbon construction strategies, and future studies should focus on scaling up this approach, exploring additional nanomaterials, and conducting long-term durability assessments. Acknowledgements I would like to express my sincere gratitude to my hardworking research team and acknowledged academic colleagues, whose ongoing support and spirit of teamwork were important for effective conclusion of this research project. Author contributions M.H.D. performed experiments and investigations, M.A.M. and D.H.K. developed software and G.K. wrote manuscript and M. Ö. supervised the projects. All authors reviewed the paper. Data availability Some or all data, models, or codes that support the findings of this study are available from the corresponding author upon reasonable request. Declarations Competing interests The authors declare no competing interests. Footnotes Publisher’s note Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations. Contributor Information Mahmood Hunar Dheyaaldin, Email: mahmood.dheyaaldin@cihanuniversity.edu.iq. Dler H. Kadir, Email: dler.kadir@su.edu.krd. References Associated Data Data Availability Statement Some or all data, models, or codes that support the findings of this study are available from the corresponding author upon reasonable request.