Synthesis of hydrazine-functionalized Polyrotaxane and formation of adaptable sliding hydrogels Authors: Sarah J. Loveland, Xinming Tong, Hung-Pang Lee, Christine L. Zhou, Fan Yang Published: 2026 ABSTRACT This work details the synthesis and characterization of Polyrotaxane-Hydrazine (PR-Hyd), a polyethylene glycol-based polymer utilized in the formation of Adaptable Sliding Hydrogels (ASG). ASG is a viscoelastic 3D cell culture system with reversible hydrazone bonds that can be leveraged to present cells with tunable stress relaxation and mechanical plasticity. ASG builds upon our lab’s previously reported Sliding Hydrogel (SG) platform which is formed via irreversible covalent crosslinking between norbornene functionalized Polyrotaxane (PR-NB) and a dithiol crosslinker. To generate PR-Hyd, we adapted and optimized the synthesis protocol for PR-NB and used proton NMR spectroscopy to quantify polymer functionality and reduce batch-to-batch variability. In addition, this work outlines our protocol for facile ASG scaffold formation using aldehyde functionalized polyethylene glycol macromers for crosslinking. Taken together, these methods enable reproducible synthesis of PR-Hyd and the fabrication of reversibly crosslinked ASG scaffolds that can be leveraged as a 3D cell niche for applications including regenerative medicine and in vitro disease modeling.•Synthesis method for Polyrotaxane-Hydrazine, a polyethylene glycol-based polymer precursor designed for forming Adaptable Sliding Hydrogels (ASG).•Characterization of polymer functionality via proton NMR spectroscopy.•Reproducible fabrication of ASG hydrogels. Specifications table Subject areaMaterials ScienceMore specific subject areaBiomaterials and tissue engineeringName of your methodSynthesis of hydrazine-functionalized Polyrotaxane and formation of adaptable sliding hydrogelsName and reference of original methodS.J. Loveland, X. Tong, M. Ayushman, Adaptable sliding hydrogels enable pericellular pocket formation while enhancing MSC chondrogenesis and survival in 3D, Bioact. Mater. 62 (2026). 10.1016/j.bioactmat.2026.03.014Resource availabilityNA Subject areaMaterials ScienceMore specific subject areaBiomaterials and tissue engineeringName of your methodSynthesis of hydrazine-functionalized Polyrotaxane and formation of adaptable sliding hydrogelsName and reference of original methodS.J. Loveland, X. Tong, M. Ayushman, Adaptable sliding hydrogels enable pericellular pocket formation while enhancing MSC chondrogenesis and survival in 3D, Bioact. Mater. 62 (2026). 10.1016/j.bioactmat.2026.03.014Resource availabilityNA Background The Adaptable Sliding Hydrogel (ASG) is a novel biomaterial scaffold designed to probe interactions between local hydrogel mechanics and cell behavior [1]. Distinct from conventional static hydrogels, ASG integrates two dynamic polymer architectures: sliding rings and reversible crosslinks. Both features can independently enhance local matrix reorganizability and facilitate nascent protein deposition, local remodeling, and mesenchymal stromal cell (MSC) differentiation [[2], [3], [4]]. Polyrotaxane backbone dynthesis The foundation of the ASG platform is a Polyrotaxane (PR) backbone composed of mechanically interlocked macrocyclic rings thread along a linear polymer chain [5,6]. Much like beads on a necklace, these rings slide dynamically along the polymer backbone, and bulky end-capping groups are used to prevent rings from unthreading. While PR can be generated from a range of different linear backbones such as polyethylene glycol (PEG), polyurethane, or polyamide and ring structures including cyclodextrins (CDs), cucurbiturils, or crown ethers, the increased solubility and facile assembly of PEG and α-CD based PR make it the most common choice for biological applications [[7], [8], [9]]. PR generated from PEG and α-CD also displays excellent biocompatibility, resists cell-based degradation, and contains functional group handles for crosslinking motif incorporation. Once end-capped, PR can be modified to improve aqueous solubility and to add functional groups that incorporate biochemical ligands or facilitate interchain crosslinking [2]. Specifically, we demonstrated that alkyne handles and hydroxypropyl groups can be conjugated onto the α-CD rings to disrupt crystalline packing and enable downstream click chemistry [10,11]. Evolution from permanent to adaptable covalent crosslinks Previous work from our lab on sliding hydrogels (SG) utilized copper-catalyzed azide-alkyne cycloaddition (CuAAC) click chemistry to add norbornene functional groups to alkyne-functionalized α-CD rings thread on PEG chains (PR-Alkyne) to form PR-Norbornene (PR-NB) [10,11]. PR-NB was subsequently crosslinked via thiol-ene click reactions with linear PEG-dithiols. The resulting SG provided cells with a more permissible local microenvironment when compared to conventional static hydrogels by facilitating cell-mediated local niche reorganization and cytoskeletal network reorganization [11]. To further enhance network mobility and permissibility, we sought to replace the irreversible covalent crosslinks of SG with reversible hydrazone bonds. By grafting hydrazine onto the PR-alkyne backbone, we obtained PR-Hyd which can be crosslinked with aldehyde-functionalized macromers. The resulting hydrogels exhibit time- and strain-dependent behaviors including stress relaxation and irreversible plasticity which are characteristic properties of viscoelastic hydrogel systems such as collagen, alginate and reversibly crosslinked hyaluronic acid hydrogels [4,[12], [13], [14], [15]]. In the ASG system, the chemical structure of the aldehyde crosslinker can be tuned to modulate bond kinetics and to modulate bulk hydrogel mechanical properties such as stress relaxation and plasticity [3,16]. ASG serves as a versatile and unique 3D cell niche for probing the effects of sliding rings and tunable bond kinetics on cell fate. In this work, we provide detailed step-by-step methods for the synthesis and characterization of PR-Hyd, enabling reproducible fabrication of hydrazone-based hydrogels for 3D cell culture with highly tunable mechanical properties. Method details Synthesis of PR Polyrotaxane (PR) synthesis has been reported previously, but reagent concentrations and reaction conditions have been updated and optimized in this work to yield polymers that form hydrogels with consistent mechanical properties [10,11]. Materials -35 kDa linear polyethylene glycol (PEG): Sigma-Aldrich 81310-2,2,6,6-tetramethylpiperidine 1-oxyl (TEMPO)-sodium bromide (NaBr)-acetonitrile-sodium hypochlorite (NaClO)-ethanol-hydrochloric acid (HCl)-dichloromethane (DCM)-hexanes-sodium sulfate (Na2SO4)-alpha cyclodextrin (α-CD): Biosynth OC06644-1-adamantanamine hydrochloride-N,N-dimethylformamide (DMF)-N,N-diisopropylethylamine (DIPEA)-benzotriazole-1-yloxytripyrrolidinophosphonium hexafluorophosphate (PyBOP)-chloroform-d (CDCl3)-dimethyl sulfoxide-d6 (DMSO) -35 kDa linear polyethylene glycol (PEG): Sigma-Aldrich 81310 35 kDa linear polyethylene glycol (PEG): Sigma-Aldrich 81310 -2,2,6,6-tetramethylpiperidine 1-oxyl (TEMPO) 2,2,6,6-tetramethylpiperidine 1-oxyl (TEMPO) -sodium bromide (NaBr) sodium bromide (NaBr) -acetonitrile acetonitrile -sodium hypochlorite (NaClO) sodium hypochlorite (NaClO) -ethanol ethanol -hydrochloric acid (HCl) hydrochloric acid (HCl) -dichloromethane (DCM) dichloromethane (DCM) -hexanes hexanes -sodium sulfate (Na2SO4) sodium sulfate (Na2SO4) -alpha cyclodextrin (α-CD): Biosynth OC06644 alpha cyclodextrin (α-CD): Biosynth OC06644 -1-adamantanamine hydrochloride 1-adamantanamine hydrochloride -N,N-dimethylformamide (DMF) N,N-dimethylformamide (DMF) -N,N-diisopropylethylamine (DIPEA) N,N-diisopropylethylamine (DIPEA) -benzotriazole-1-yloxytripyrrolidinophosphonium hexafluorophosphate (PyBOP) benzotriazole-1-yloxytripyrrolidinophosphonium hexafluorophosphate (PyBOP) -chloroform-d (CDCl3) chloroform-d (CDCl3) -dimethyl sulfoxide-d6 (DMSO) dimethyl sulfoxide-d6 (DMSO) Equipment -Glassware-Separatory funnel-Rotary evaporator-Vacuum chamber-Centrifuge-1H-NMR spectrometer-Standard microwave-NMR tubes -Glassware Glassware -Separatory funnel Separatory funnel -Rotary evaporator Rotary evaporator -Vacuum chamber Vacuum chamber -Centrifuge Centrifuge -1H-NMR spectrometer 1H-NMR spectrometer -Standard microwave Standard microwave -NMR tubes NMR tubes Step-by-step methods Oxidation of 35kDa-PEG to 35kDa-PEG-COOH (Fig. 1A) First, 20 g of 35kDa-PEG was dissolved in 200 mL DI water. In 1 mL acetonitrile, 150 mg TEMPO was dissolved and added to the PEG solution. 150 mg of NaBr was then added and fully dissolved. Next, 30 mL of NaClO was added to the mixture, and the reaction was left stirring for 30 minutes at room temperature (RT). 10 mL of ethanol was added to quench the oxidation reaction, and the pH was adjusted to 1 using concentrated HCl. To extract the oxidized 35kDa-PEG-COOH, 100 mL DCM was added to the aqueous solution, mixed, and separated using a separatory funnel. The organic layer enriched in 35kDa-PEG-COOH was collected, and the extraction was repeated 3 more times until the organic phase was no longer viscous. The combined organic phase was dried with Na2SO4 and concentrated using a rotary evaporator. The product was then precipitated in ∼250 mL ice-cooled hexanes, and the solid was collected and left to dry in a vacuum chamber overnight. 1H-NMR validation was performed using CDCl3 as a solvent (Fig. 1B-C).Fig. 1Synthesis and characterization of Polyrotaxane (PR). A) Reaction schematic of 35kDa-PEG oxidation with TEMPO. B) 1H-NMR validation of complete oxidation is shown with the absence of a TAIC peak at 4.40 ppm. C) Peak assignments for 35kDa-PEG-COOH. D) Outline of PPR self-assembly and end-capping. E) Reaction schematic of PPR end-capping with 1-adamantanamine. F) 1H-NMR spectrum of PR with G) assigned peaks for shown protons.Fig 1: dummy alt text Synthesis and characterization of Polyrotaxane (PR). A) Reaction schematic of 35kDa-PEG oxidation with TEMPO. B) 1H-NMR validation of complete oxidation is shown with the absence of a TAIC peak at 4.40 ppm. C) Peak assignments for 35kDa-PEG-COOH. D) Outline of PPR self-assembly and end-capping. E) Reaction schematic of PPR end-capping with 1-adamantanamine. F) 1H-NMR spectrum of PR with G) assigned peaks for shown protons. Pseudo-Polyrotaxane (PPR) (Fig. 1D) To form PPR, 15 g of 35kDa-PEG-COOH was dissolved in 100 mL of DI water. In a separate beaker, 33 g of α-CD were added to 220 mL DI water and warmed in a microwave until fully dissolved. The solutions were mixed and left stirring on low at R.T. overnight (Fig. 2A). The next day, the solution became thick, milky, and cloudy and was frozen in 50 mL Falcon tubes before lyophilization (Fig. 2B-C).Fig. 2Synthesis and work-up outline for Polyrotaxane (PR). A) α-CD and 35kDa-PEG-COOH are dissolved and combined in DI water and left stirring overnight at room temperature (RT). B) The solution should be thick and milky the next day with a solid layer on top. C) The Pseudo-Polyrotaxane (PPR) is transferred to 50 mL tubes and frozen before lyophilization to yield a white powder. D) The PPR is crushed and separated into a light, fluffy consistency. E) Coupling reagents and solvent are added to the mixture, and it is patted down flat. A thick stir bar is added, and stirring is set to the lowest setting overnight at RT. F) The solution should be thinner and more flowable before proceeding. G) A 4–5x volume of acetonitrile is added, the solid is collected, and repeated water washing is carried out. H) PR is frozen and lyophilized before use in the synthesis of PR-Alkyne.Fig 2: dummy alt text Synthesis and work-up outline for Polyrotaxane (PR). A) α-CD and 35kDa-PEG-COOH are dissolved and combined in DI water and left stirring overnight at room temperature (RT). B) The solution should be thick and milky the next day with a solid layer on top. C) The Pseudo-Polyrotaxane (PPR) is transferred to 50 mL tubes and frozen before lyophilization to yield a white powder. D) The PPR is crushed and separated into a light, fluffy consistency. E) Coupling reagents and solvent are added to the mixture, and it is patted down flat. A thick stir bar is added, and stirring is set to the lowest setting overnight at RT. F) The solution should be thinner and more flowable before proceeding. G) A 4–5x volume of acetonitrile is added, the solid is collected, and repeated water washing is carried out. H) PR is frozen and lyophilized before use in the synthesis of PR-Alkyne. Polyrotaxane (PR) (Fig. 1E) 24 g of lyophilized PPR was added to a large beaker and broken apart until light and fluffy (Fig. 2D). In a separate flask, 4 g of 1-adamantanamine hydrochloride was dissolved in 120 mL DMF. Next, 3 mL of DIPEA was added and stirred until almost completely dissolved. Finally, 10 g of PyBOP was added and stirred until dissolved. The solution was then poured over the PPR solid, and a large stir bar was added. The resulting mixture should be thick (will not be flowable) and was packed down into the bottom of the flask and stirring was set to the slowest speed possible overnight (Fig. 2E). The stir bar should begin to move in the solution overnight. If the mixture is still very dry the next day, around 4-10 mL of DMF can be added, the solid can be patted down gently, and the reaction can be left again overnight. The solution in this case was found to become thin and flowable but not completely clear, and the PR product was then collected as follows (Fig. 2F). First, the suspension was poured into a 4-5x volume of acetonitrile to precipitate the PR product. This mixture was aliquoted into 50 mL Falcon tubes and centrifuged at 600g for 3 minutes. The white solid settled at the bottom of the tube, and the supernatant was poured off the top. The solid was then mixed with hot (∼80-90°C) 200 mL DI water (Fig. 2G). If the polymer mixture fully dissolves in the hot water, the endcapping reaction was unsuccessful: PR is insoluble in water and can be collected as a solid via centrifugation while PEG and free α-CD will dissolve during washing. The washing step was repeated two more times, and the solid was frozen and lyophilized (Fig. 2H). Validation was conducted using 1H-NMR spectroscopy in DMSO (Fig. 1F-G). 1H-NMR spectroscopy was also used to quantify α-CD ring coverage along the PEG backbone, as detailed in the method validation section. Under these reaction conditions, the final PR-Hydrazine (PR-Hyd) product had a ring coverage of approximately 8-10%. Of note, ring coverage after initial PR assembly was typically higher at 15-20%, as quantified by 1H-NMR. The decrease in coverage is likely due to residual free α-CD rings that were not fully removed during water washing. Synthesis of PR-Alkyne Here, we detail the updates that have been made to our previous synthesis methods for PR-alkyne (Fig. 3A-B) [10].Fig. 3Synthesis and characterization of PR-alkyne from PR. A) Reaction schematic of PR-alkyne synthesis and B) structure illustration. C) 1HNMR spectrum of PR-alkyne with assigned peaks.Fig 3: dummy alt text Synthesis and characterization of PR-alkyne from PR. A) Reaction schematic of PR-alkyne synthesis and B) structure illustration. C) 1HNMR spectrum of PR-alkyne with assigned peaks. Materials -glycidyl propargyl ether: Sigma 50062-propylene oxide-sodium hydroxide (NaOH)-deuterium oxide (D2O)-12-14 kDa dialysis tubing: Spectrum 08-667E -glycidyl propargyl ether: Sigma 50062 glycidyl propargyl ether: Sigma 50062 -propylene oxide propylene oxide -sodium hydroxide (NaOH) sodium hydroxide (NaOH) -deuterium oxide (D2O) deuterium oxide (D2O) -12-14 kDa dialysis tubing: Spectrum 08-667E 12-14 kDa dialysis tubing: Spectrum 08-667E Equipment -1H-NMR spectrometer-Lyophilizer -1H-NMR spectrometer 1H-NMR spectrometer -Lyophilizer Lyophilizer Step-by-step methods PR-Alkyne 5 g of PR were dissolved in 250 mL of 1M NaOH and cooled on ice. 2.5 mL of glycidyl propargyl ether were added to the solution and stirred for at least 3 hours until the solution became clear. The ice bath was refreshed, the solution was once again cooled, and 1.25 mL of glycidyl propargyl ether were added and left overnight to react. The next day, the solution was cooled on ice before 100 mL cold propylene oxide were added and left to react for at least 3 hours. The solution was once more cooled, and an additional 100 mL cold propylene oxide were added and left to react overnight. The solution was then neutralized and dialyzed against DI water in 12-14 kDa molecular weight cutoff dialysis tubing then frozen and lyophilized. Validation was conducted via 1H-NMR spectroscopy in D2O (Fig. 3C). Synthesis of PR-Hydrazine (Fig. 4A-B) PR-Hydrazine (PR-Hyd) is a novel advancement to the sliding hydrogel polymer that allows for reversible crosslinking. To functionalize PR-Alkyne, copper-catalyzed azide-alkyne cycloaddition (CuAAC) click chemistry was used to attach a tri-boc-hydrazine-azidopropyl amide bifunctional small molecule. After deprotection of the boc-protected PR-Hyd, the final polymer is characterized and can be used for hydrogel formation. Materials -3-azido-1-propanamine:○Commercial source: Sigma-Aldrich 7620169-tri-boc-hydrazinoacetic acid:○Previously reported synthesis method: [17]○Commercial source: Sigma-Aldrich 68972-DCM-1-ethyl-3-(3-dimethylaminopropyl)carbodiimide (EDC HCl)-4-dimethylaminopyridine (DMAP)-HCl-brine-Na2SO4-silica: Millipore 1077341000-ethyl acetate (EtOAc)-hexanes-methanol (MeOH)-sodium ascorbate-N,N,N′,N′′,N′′-pentamethyldiethylenetriamine (PMDETA)-copper sulfate (CuSO4)-ethylenediaminetetraacetic acid (EDTA)-Dialysis tubing: Spectrum 08-667E -3-azido-1-propanamine:○Commercial source: Sigma-Aldrich 7620169 3-azido-1-propanamine:○Commercial source: Sigma-Aldrich 7620169 ○Commercial source: Sigma-Aldrich 7620169 Commercial source: Sigma-Aldrich 7620169 -tri-boc-hydrazinoacetic acid:○Previously reported synthesis method: [17]○Commercial source: Sigma-Aldrich 68972 tri-boc-hydrazinoacetic acid:○Previously reported synthesis method: [17]○Commercial source: Sigma-Aldrich 68972 ○Previously reported synthesis method: [17] Previously reported synthesis method: [17] ○Commercial source: Sigma-Aldrich 68972 Commercial source: Sigma-Aldrich 68972 -DCM DCM -1-ethyl-3-(3-dimethylaminopropyl)carbodiimide (EDC HCl) 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide (EDC HCl) -4-dimethylaminopyridine (DMAP) 4-dimethylaminopyridine (DMAP) -HCl HCl -brine brine -Na2SO4 Na2SO4 -silica: Millipore 1077341000 silica: Millipore 1077341000 -ethyl acetate (EtOAc) ethyl acetate (EtOAc) -hexanes hexanes -methanol (MeOH) methanol (MeOH) -sodium ascorbate sodium ascorbate -N,N,N′,N′′,N′′-pentamethyldiethylenetriamine (PMDETA) N,N,N′,N′′,N′′-pentamethyldiethylenetriamine (PMDETA) -copper sulfate (CuSO4) copper sulfate (CuSO4) -ethylenediaminetetraacetic acid (EDTA) ethylenediaminetetraacetic acid (EDTA) -Dialysis tubing: Spectrum 08-667E Dialysis tubing: Spectrum 08-667E Equipment -Hot plate-Chromatography column-Rotovap-Lyophilizer -Hot plate Hot plate -Chromatography column Chromatography column -Rotovap Rotovap -Lyophilizer Lyophilizer Step-by-step methods Tri-boc-hydrazine-azidopropyl amide Together, 2 g of tri-boc-hydrazinoacetic acid and 1.34 g of 3-azido-1-propanamine were combined in 100 mL DCM. Next, 2.93 g of EDC HCl were added before 0.065 g of DMAP. The solution was left stirring overnight. To purify the product, the solution is washed with 100 mL of 0.1 N HCl twice and with 100 mL of brine once. After drying with Na2SO4, the solvent was evaporated and a short silica gel column with 1:1 EtOAc:hexanes was used to purify the product. Boc-protected PR-Hyd First, 1 g PR-alkyne was dissolved in 18 mL of a 1:1 mixture of MeOH and DI water. In 1 mL of MeOH, 0.47 g of tri-boc-hydrazine-azidopropyl amide were dissolved and subsequently added to the PR-alkyne solution. 1.5 mL of a 10 wt% sodium ascorbate solution in DI water and 50 µL of a 10 wt% stock solution of CuSO4 in PMDETA (0.48 M) were also added to the reaction mixture and stirred at R.T. overnight. The next day, 1 mL of EDTA (1 M) was added and stirred for 5 minutes. The resulting solution was then dialyzed against DI water for at least 24 hours. Finally, the solution was frozen and lyophilized. Validation of the product is done using 1H-NMR spectroscopy (Fig. 4C,E-F).Fig. 4Synthesis and characterization of PR-hydrazine. A) Reaction schematic of copper-catalyzed alkyne azide cycloaddition (CuAAC) click chemistry to synthesize boc-protected PR-Hydrazine. B) Illustration of polymer functionalization. C) 1HNMR spectrum of boc-protected PR-Hydrazine and D) PR-Hydrazine with E-G) peak assignments.Fig 4: dummy alt text Synthesis and characterization of PR-hydrazine. A) Reaction schematic of copper-catalyzed alkyne azide cycloaddition (CuAAC) click chemistry to synthesize boc-protected PR-Hydrazine. B) Illustration of polymer functionalization. C) 1HNMR spectrum of boc-protected PR-Hydrazine and D) PR-Hydrazine with E-G) peak assignments. Importantly, the mass of tri-boc-hydrazine-azidopropyl amide added can be adjusted. If a significant quantity of unreacted alkyne is present and the hydrazine functionality is less than ∼ 0.4 hydrazine/α-CD ring, increase the amount of tri-boc-hydrazine-azidopropyl amide. PR-Hyd In DI water, 1 g of boc-protected PR-Hyd, 1 mL of EDTA (1M), and 6 mL of 12 N HCl were combined and stirred at 40°C for at least 30 minutes. The polymer became soluble as deprotection occurred. When the solution was clear and all polymer had dissolved, the reaction was stopped. The solution’s pH was brought to 5-6 with HCl before dialysis against water for at least 24 hours. After freezing and vacuum drying, the product was validated via 1H-NMR spectroscopy (Fig. 4D, G). A ratio of 0.47 g of tri-boc-hydrazine-azidopropyl amide to 1 g of PR-alkyne with a functionality of 1-2 alkyne per α-CD ring and 8-10% coverage yielded PR-Hyd with approximately 0.5 hydrazine per ring, as quantified using 1H-NMR spectroscopy. Formation of PR-Hyd-based hydrogels Using 1H-NMR spectroscopy, the functionality of PR-Hyd can be quantified as the weight of polymer per one mol of hydrazine functional groups. The calculations are summarized in Table 1. To form hydrogels, 10kDa-8-arm-PEG aliphatic aldehyde (AA) and benzaldehyde (BA) are used as crosslinkers. As outlined in previous work, tuning the ratio of AA:BA crosslinks allows for control over the stress relaxation and plasticity of the resulting hydrogels [1,3,16]. AA-based crosslinks are more dynamic than BA-based crosslinks and result in faster stress relaxing hydrogels due to more rapid molecular reorganization under applied stress. For gel formulation, the hydrazine:aldehyde ratio was set to a 1:1 molar ratio to ensure stable network formation. In our work, 10kDa-8-arm-PEG-aliphatic aldehyde (8-arm-PEG-AA) and 10kDa-8-arm-PEG-benzaldehyde (8-arm-PEG-BA) crosslinkers were used and synthesized as previously described [3,18]. For polymer precursor solutions, PR-Hyd stock solutions are made at 10 wt% due to high viscosity while 8-arm-PEG-aldehyde solutions are made at 20 wt%.Table 1Values for PR, PR-alkyne, and PR-Hyd coverage and functionality calculations.Table 1: dummy alt textValues for calculationsValueUnitsPolymer molecular weight (MW)35,000g/molPEG monomer MW44.05g/molHydroxyl end-group MW18.02g/molNumber PEG monomers per chain794monomersPEG monomers covered per α-CD ring2monomersNumber α-CD per PEG chain at 100% coverage397α-CDPEG protons covered by one α-CD ring8protonsα-CD protons between δ 3.80–3.3536protonsTotal protons per α-CD ring60protons Table 1Values for PR, PR-alkyne, and PR-Hyd coverage and functionality calculations.Table 1: dummy alt textValues for calculationsValueUnitsPolymer molecular weight (MW)35,000g/molPEG monomer MW44.05g/molHydroxyl end-group MW18.02g/molNumber PEG monomers per chain794monomersPEG monomers covered per α-CD ring2monomersNumber α-CD per PEG chain at 100% coverage397α-CDPEG protons covered by one α-CD ring8protonsα-CD protons between δ 3.80–3.3536protonsTotal protons per α-CD ring60protons Values for PR, PR-alkyne, and PR-Hyd coverage and functionality calculations. Materials -PR-Hyd-8-arm-PEG-AA (10kDa) and 8-arm-PEG-BA (10kDa) synthesized as previously described [3,18]○DCM○8-arm 10kDa PEG (JenKem)○(diacetoxyiodo)benzene (DAIB)○TEMPO○4-formyl benzoic acid○N,N’-Diisopropylcarbodiimide (DIC)○DMAP○diethyl ether○1 kDa MWCO dialysis tubing: Spectrum 08-680-Teflon tape (3M 5480 PTFE film tape)-Biopsy punches-1 N HCl-1 N NaOH-PBS -PR-Hyd PR-Hyd -8-arm-PEG-AA (10kDa) and 8-arm-PEG-BA (10kDa) synthesized as previously described [3,18]○DCM○8-arm 10kDa PEG (JenKem)○(diacetoxyiodo)benzene (DAIB)○TEMPO○4-formyl benzoic acid○N,N’-Diisopropylcarbodiimide (DIC)○DMAP○diethyl ether○1 kDa MWCO dialysis tubing: Spectrum 08-680 8-arm-PEG-AA (10kDa) and 8-arm-PEG-BA (10kDa) synthesized as previously described [3,18]○DCM○8-arm 10kDa PEG (JenKem)○(diacetoxyiodo)benzene (DAIB)○TEMPO○4-formyl benzoic acid○N,N’-Diisopropylcarbodiimide (DIC)○DMAP○diethyl ether○1 kDa MWCO dialysis tubing: Spectrum 08-680 ○DCM DCM ○8-arm 10kDa PEG (JenKem) 8-arm 10kDa PEG (JenKem) ○(diacetoxyiodo)benzene (DAIB) (diacetoxyiodo)benzene (DAIB) ○TEMPO TEMPO ○4-formyl benzoic acid 4-formyl benzoic acid ○N,N’-Diisopropylcarbodiimide (DIC) N,N’-Diisopropylcarbodiimide (DIC) ○DMAP DMAP ○diethyl ether diethyl ether ○1 kDa MWCO dialysis tubing: Spectrum 08-680 1 kDa MWCO dialysis tubing: Spectrum 08-680 -Teflon tape (3M 5480 PTFE film tape) Teflon tape (3M 5480 PTFE film tape) -Biopsy punches Biopsy punches -1 N HCl 1 N HCl -1 N NaOH 1 N NaOH -PBS PBS Equipment -Incubator at 37°C-Vortex mixer -Incubator at 37°C Incubator at 37°C -Vortex mixer Vortex mixer Step-by-step methods 8-arm-PEG-AA synthesis [18] To a solution of 100 mL DCM, 5 g 8-arm 10kDa PEG, 3.87 g DAIB (3 eq), and 0.125 g TEMPO (0.2 eq) were added. This reaction was stirred overnight at room temperature. The solution was then added dropwise into cooled diethyl ether, and the resulting precipitate was collected, dissolved in deionized water, and dialyzed against DI water for 2 days. 8-arm-PEG-BA synthesis [3] In 100 mL DCM, 5 g of 8-arm 10kDa PEG was dissolved and combined with 1.2 g 4-formylbenzoic acid (2 eq), 0.147 g DMAP (0.3 eq), and 1.5 g DIC (3 eq). The reaction was left stirring overnight before the product was precipitated in cooled diethyl ether and dialyzed against deionized water for 2 days. Hydrogel precursor solutions of PR-Hyd are made as follows (Fig. 5A):1.Example: 500 µL of a 10 wt% stock solution2.Weigh 0.05 g PR-Hydrazine3.Add 250 µL PBS4.Add 50 µL 1N HCl and wait until polymer is almost completely dissolved5.Neutralize with 1 N NaOH and bring total volume to 500 µL with PBS, but take care to not bring the pH above 7.46.For 8-arm-PEG-AA and 8-arm-PEG-BA stock precursors, dissolve at 20 wt% in PBS and neutralizeFig. 5Step-by-step protocol for polymer dissolution and hydrogel assembly optimized for ASG. A) PR-Hydrazine is first dissolved in PBS and ∼0.2 N HCl before neutralization. B) Hydrogels are formed by pipetting an 8-arm-PEG-aldehyde solution onto a Teflon-coated glass slide and adding 2 spacers that are 1 mm (stacked height is 2 mm) on each side (step 1). PR-Hydrazine is combined with PBS (or cells and media for cellular encapsulations) and mixed quickly with the aldehyde (steps 2–3). A top Teflon-coated slide is placed on top on the spacers and gelation occurs over 20 min at 37 °C (step 4). The top slide is carefully removed, and a biopsy punch is then used to punch out individual hydrogel scaffolds (step 5–6).Fig 5: dummy alt text 1.Example: 500 µL of a 10 wt% stock solution Example: 500 µL of a 10 wt% stock solution 2.Weigh 0.05 g PR-Hydrazine Weigh 0.05 g PR-Hydrazine 3.Add 250 µL PBS Add 250 µL PBS 4.Add 50 µL 1N HCl and wait until polymer is almost completely dissolved Add 50 µL 1N HCl and wait until polymer is almost completely dissolved 5.Neutralize with 1 N NaOH and bring total volume to 500 µL with PBS, but take care to not bring the pH above 7.4 Neutralize with 1 N NaOH and bring total volume to 500 µL with PBS, but take care to not bring the pH above 7.4 6.For 8-arm-PEG-AA and 8-arm-PEG-BA stock precursors, dissolve at 20 wt% in PBS and neutralize For 8-arm-PEG-AA and 8-arm-PEG-BA stock precursors, dissolve at 20 wt% in PBS and neutralize Step-by-step protocol for polymer dissolution and hydrogel assembly optimized for ASG. A) PR-Hydrazine is first dissolved in PBS and ∼0.2 N HCl before neutralization. B) Hydrogels are formed by pipetting an 8-arm-PEG-aldehyde solution onto a Teflon-coated glass slide and adding 2 spacers that are 1 mm (stacked height is 2 mm) on each side (step 1). PR-Hydrazine is combined with PBS (or cells and media for cellular encapsulations) and mixed quickly with the aldehyde (steps 2–3). A top Teflon-coated slide is placed on top on the spacers and gelation occurs over 20 min at 37 °C (step 4). The top slide is carefully removed, and a biopsy punch is then used to punch out individual hydrogel scaffolds (step 5–6). Hydrogel formation: Hydrogels are typically stable and can be formed at a final polymer concentration between 4 and 9 wt% depending on functionality. Going below that range may result in gels that are unstable over time while going above may be challenging due to the rapid gelation. Cell solutions and excess PBS should be included in the final volume during calculations. Keep all precursor solutions on ice to slow gelation process and allow for proper mixing (Fig. 5B).1.Combine PR-Hyd and PBS and vortexa.Optional: add cells and pipette thoroughly to mix2.Dispense aldehyde stock solution onto Teflon-coated slides3.Add the spacers and top Teflon slide4.Combine the precursor solution containing PR-Hyd and PBS (± cells) with the aldehyde on the slide by pipetting carefully up and down, the solution will start to increase in viscosity as gelation begins5.Place in incubator or at 37°C for 20 minutes6.Punch out hydrogels using biopsy punch of desired size7.Transfer to cell culture media if applicable 1.Combine PR-Hyd and PBS and vortexa.Optional: add cells and pipette thoroughly to mix Combine PR-Hyd and PBS and vortexa.Optional: add cells and pipette thoroughly to mix a.Optional: add cells and pipette thoroughly to mix Optional: add cells and pipette thoroughly to mix 2.Dispense aldehyde stock solution onto Teflon-coated slides Dispense aldehyde stock solution onto Teflon-coated slides 3.Add the spacers and top Teflon slide Add the spacers and top Teflon slide 4.Combine the precursor solution containing PR-Hyd and PBS (± cells) with the aldehyde on the slide by pipetting carefully up and down, the solution will start to increase in viscosity as gelation begins Combine the precursor solution containing PR-Hyd and PBS (± cells) with the aldehyde on the slide by pipetting carefully up and down, the solution will start to increase in viscosity as gelation begins 5.Place in incubator or at 37°C for 20 minutes Place in incubator or at 37°C for 20 minutes 6.Punch out hydrogels using biopsy punch of desired size Punch out hydrogels using biopsy punch of desired size 7.Transfer to cell culture media if applicable Transfer to cell culture media if applicable Method validation 1.Validation of PEG oxidation and PR synthesis is done via 1H-NMR spectroscopy.1.1.To determine if oxidation of the hydroxyl end groups was complete, 1H-NMR was used on a polymer sample with and without trichloroacetyl isocyanate (TAIC). TAIC can be used as an in situ derivatizing agent that rapidly reacts with hydroxyl or amine functional groups, causing a significant downfield shift in the nearby PEG protons that can be observed at ∼4.40 ppm in chloroform-d (CDCl3) (Fig. 1B-C).1.2.To quantify ring coverage along the PEG backbone, PR was dissolved in dimethyl sulfoxide-d6 (DMSO), and a spectrum was obtained (Fig. 1F-G).1.3.35kDa-PEG-COOH: 1H-NMR (500 MHz, CDCl3) δ: ∼3.65 (∼3182H).1.435kDa-PEG-COOH + TAIC: 1H-NMR (500 MHz, CDCl3) δ: ∼3.65 (∼3182H), δ: 4.40 (t, 2H) if unreacted hydroxyl is present.1.5.PR: 1H-NMR (500 MHz, DMSO) δ: ∼5.75-5.35 (12 Ha), 4.80 (6 Hb) 4.4 (6 Hc), ∼3.80-3.35 (36 Hd + 48 *He).1.6.*He changes slightly between polymer batches, and it is important to check 1H-NMR every time a new batch is made. For the spectrum shown in Fig. 1F, Hd + He was 84, thus He was 48.1.7.Polyrotaxane coverage calculations: relevant values included in Table 1. 1. Coverage from 1H-NMR:a. α-CD protons: 60 H total (12 Ha, 6 Hb, 6 Hc, 36 Hd)b. PEG protons: subtract 36 Hd from integration at ∼3.80-3.35 to calculate PEG He per α-CD= 84 – 36 Hd= 48 PEG He per α-CD ringc. % coverage = 8 / (PEG He per α-CD) * 100%= 8 / 48= 0.167 * 100% = 16.7% coveraged. The number of α-CD per PEG chain with full coverage is half the number of PEG monomers (∼794/2 = 397), so the actual number = 397 * 0.167 = ∼ 66 α-CD per chain 2.Validation of PR-alkyne functionality is done via 1H-NMR spectroscopy (Fig. 3C)2.1.To determine the alkyne functionality, the integration of the 6 Ha α-CD protons was normalized. The alkyne peak at 4.30 thus represented the number of alkyne groups per ring. For hydroxypropyl functionality, the methyl He peak integration was divided by three to calculate the number of hydroxypropyl groups incorporated per ring. In our experience, ∼1-2 alkyne per ring and >3 hydroxypropyl groups per ring yielded the best results for subsequent reactions, though these can be modified depending on the desired final functionality. In the representative example shown (Fig. 3C), the α-CD rings were functionalized with 2.1 alkyne and ∼3.9 hydroxypropyl groups per ring. Given a ring coverage of 10.8% and a theoretical maximum of 397 rings per PR chain for 100% coverage (Table 1), each PR contains ∼43 rings. Thus, this batch of polymer contains approximately 90 alkyne groups per macromer.2.2.PR-Alkyne: 1H-NMR (500 MHz, DMSO) δ: ∼5.35-5.00 (6 Ha), 4.30 (1 Hb), 4.2-3.3 (36 Hc + 74 *Hd), 1.20 (24 *He).2.3.*Values vary between batches of polymer depending on glycidyl propargyl ether and propylene oxide incorporation.3.Validation of final PR-Hyd functionality and boc-deprotection are confirmed via 1H-NMR spectroscopy (Fig. 4C-G)3.1.The 6 Hb α-CD protons were again used for normalization. The peak at 8.09 ppm corresponded to the triazole proton (Ha) that appeared after CuAAC crosslinking and was therefore used to quantify the number of hydrazine molecules per α-CD ring.3.2.Boc-protected PR-Hyd: 1H-NMR (500 MHz, DMSO) δ: 8.09 (1 Ha), ∼5.10-4.60 (6 Hb), ∼4.00-3.02 (36 Hc + 42 *Hd), 1.40 (27 He), 1.01 (12 *Hf).3.3.PR-Hyd: 1H-NMR (500 MHz, DMSO) δ: 8.09 (1 Ha), ∼5.35-5.00 (6 Hb), ∼4.20-3.30 (36 Hc + 76 *Hd), 1.20 (12 *He).3.4.In the representative spectrum shown (Fig. 4D), the polymer exhibited an α-CD coverage of 10.5% with a functionality of 0.4 hydrazine per ring. This equates to approximately 42 rings and 16 hydrazine functional groups per macromer. Notably, values marked with asterisks vary between synthesis batches and should be quantified for each new batch of polymer. 1.Validation of PEG oxidation and PR synthesis is done via 1H-NMR spectroscopy.1.1.To determine if oxidation of the hydroxyl end groups was complete, 1H-NMR was used on a polymer sample with and without trichloroacetyl isocyanate (TAIC). TAIC can be used as an in situ derivatizing agent that rapidly reacts with hydroxyl or amine functional groups, causing a significant downfield shift in the nearby PEG protons that can be observed at ∼4.40 ppm in chloroform-d (CDCl3) (Fig. 1B-C).1.2.To quantify ring coverage along the PEG backbone, PR was dissolved in dimethyl sulfoxide-d6 (DMSO), and a spectrum was obtained (Fig. 1F-G).1.3.35kDa-PEG-COOH: 1H-NMR (500 MHz, CDCl3) δ: ∼3.65 (∼3182H).1.435kDa-PEG-COOH + TAIC: 1H-NMR (500 MHz, CDCl3) δ: ∼3.65 (∼3182H), δ: 4.40 (t, 2H) if unreacted hydroxyl is present.1.5.PR: 1H-NMR (500 MHz, DMSO) δ: ∼5.75-5.35 (12 Ha), 4.80 (6 Hb) 4.4 (6 Hc), ∼3.80-3.35 (36 Hd + 48 *He).1.6.*He changes slightly between polymer batches, and it is important to check 1H-NMR every time a new batch is made. For the spectrum shown in Fig. 1F, Hd + He was 84, thus He was 48.1.7.Polyrotaxane coverage calculations: relevant values included in Table 1. Validation of PEG oxidation and PR synthesis is done via 1H-NMR spectroscopy.1.1.To determine if oxidation of the hydroxyl end groups was complete, 1H-NMR was used on a polymer sample with and without trichloroacetyl isocyanate (TAIC). TAIC can be used as an in situ derivatizing agent that rapidly reacts with hydroxyl or amine functional groups, causing a significant downfield shift in the nearby PEG protons that can be observed at ∼4.40 ppm in chloroform-d (CDCl3) (Fig. 1B-C).1.2.To quantify ring coverage along the PEG backbone, PR was dissolved in dimethyl sulfoxide-d6 (DMSO), and a spectrum was obtained (Fig. 1F-G).1.3.35kDa-PEG-COOH: 1H-NMR (500 MHz, CDCl3) δ: ∼3.65 (∼3182H).1.435kDa-PEG-COOH + TAIC: 1H-NMR (500 MHz, CDCl3) δ: ∼3.65 (∼3182H), δ: 4.40 (t, 2H) if unreacted hydroxyl is present.1.5.PR: 1H-NMR (500 MHz, DMSO) δ: ∼5.75-5.35 (12 Ha), 4.80 (6 Hb) 4.4 (6 Hc), ∼3.80-3.35 (36 Hd + 48 *He).1.6.*He changes slightly between polymer batches, and it is important to check 1H-NMR every time a new batch is made. For the spectrum shown in Fig. 1F, Hd + He was 84, thus He was 48.1.7.Polyrotaxane coverage calculations: relevant values included in Table 1. 1.1.To determine if oxidation of the hydroxyl end groups was complete, 1H-NMR was used on a polymer sample with and without trichloroacetyl isocyanate (TAIC). TAIC can be used as an in situ derivatizing agent that rapidly reacts with hydroxyl or amine functional groups, causing a significant downfield shift in the nearby PEG protons that can be observed at ∼4.40 ppm in chloroform-d (CDCl3) (Fig. 1B-C). To determine if oxidation of the hydroxyl end groups was complete, 1H-NMR was used on a polymer sample with and without trichloroacetyl isocyanate (TAIC). TAIC can be used as an in situ derivatizing agent that rapidly reacts with hydroxyl or amine functional groups, causing a significant downfield shift in the nearby PEG protons that can be observed at ∼4.40 ppm in chloroform-d (CDCl3) (Fig. 1B-C). 1.2.To quantify ring coverage along the PEG backbone, PR was dissolved in dimethyl sulfoxide-d6 (DMSO), and a spectrum was obtained (Fig. 1F-G). To quantify ring coverage along the PEG backbone, PR was dissolved in dimethyl sulfoxide-d6 (DMSO), and a spectrum was obtained (Fig. 1F-G). 1.3.35kDa-PEG-COOH: 1H-NMR (500 MHz, CDCl3) δ: ∼3.65 (∼3182H). 35kDa-PEG-COOH: 1H-NMR (500 MHz, CDCl3) δ: ∼3.65 (∼3182H). 1.435kDa-PEG-COOH + TAIC: 1H-NMR (500 MHz, CDCl3) δ: ∼3.65 (∼3182H), δ: 4.40 (t, 2H) if unreacted hydroxyl is present. 35kDa-PEG-COOH + TAIC: 1H-NMR (500 MHz, CDCl3) δ: ∼3.65 (∼3182H), δ: 4.40 (t, 2H) if unreacted hydroxyl is present. 1.5.PR: 1H-NMR (500 MHz, DMSO) δ: ∼5.75-5.35 (12 Ha), 4.80 (6 Hb) 4.4 (6 Hc), ∼3.80-3.35 (36 Hd + 48 *He). PR: 1H-NMR (500 MHz, DMSO) δ: ∼5.75-5.35 (12 Ha), 4.80 (6 Hb) 4.4 (6 Hc), ∼3.80-3.35 (36 Hd + 48 *He). 1.6.*He changes slightly between polymer batches, and it is important to check 1H-NMR every time a new batch is made. For the spectrum shown in Fig. 1F, Hd + He was 84, thus He was 48. *He changes slightly between polymer batches, and it is important to check 1H-NMR every time a new batch is made. For the spectrum shown in Fig. 1F, Hd + He was 84, thus He was 48. 1.7.Polyrotaxane coverage calculations: relevant values included in Table 1. Polyrotaxane coverage calculations: relevant values included in Table 1. 1. Coverage from 1H-NMR:a. α-CD protons: 60 H total (12 Ha, 6 Hb, 6 Hc, 36 Hd)b. PEG protons: subtract 36 Hd from integration at ∼3.80-3.35 to calculate PEG He per α-CD= 84 – 36 Hd= 48 PEG He per α-CD ringc. % coverage = 8 / (PEG He per α-CD) * 100%= 8 / 48= 0.167 * 100% = 16.7% coveraged. The number of α-CD per PEG chain with full coverage is half the number of PEG monomers (∼794/2 = 397), so the actual number = 397 * 0.167 = ∼ 66 α-CD per chain 1. Coverage from 1H-NMR:a. α-CD protons: 60 H total (12 Ha, 6 Hb, 6 Hc, 36 Hd)b. PEG protons: subtract 36 Hd from integration at ∼3.80-3.35 to calculate PEG He per α-CD= 84 – 36 Hd= 48 PEG He per α-CD ringc. % coverage = 8 / (PEG He per α-CD) * 100%= 8 / 48= 0.167 * 100% = 16.7% coveraged. The number of α-CD per PEG chain with full coverage is half the number of PEG monomers (∼794/2 = 397), so the actual number = 397 * 0.167 = ∼ 66 α-CD per chain a. α-CD protons: 60 H total (12 Ha, 6 Hb, 6 Hc, 36 Hd) a. α-CD protons: 60 H total (12 Ha, 6 Hb, 6 Hc, 36 Hd) b. PEG protons: subtract 36 Hd from integration at ∼3.80-3.35 to calculate PEG He per α-CD= 84 – 36 Hd= 48 PEG He per α-CD ring b. PEG protons: subtract 36 Hd from integration at ∼3.80-3.35 to calculate PEG He per α-CD= 84 – 36 Hd= 48 PEG He per α-CD ring = 84 – 36 Hd = 84 – 36 Hd = 48 PEG He per α-CD ring = 48 PEG He per α-CD ring c. % coverage = 8 / (PEG He per α-CD) * 100%= 8 / 48= 0.167 * 100% = 16.7% coverage c. % coverage = 8 / (PEG He per α-CD) * 100%= 8 / 48= 0.167 * 100% = 16.7% coverage = 8 / 48 = 8 / 48 = 0.167 * 100% = 16.7% coverage = 0.167 * 100% = 16.7% coverage d. The number of α-CD per PEG chain with full coverage is half the number of PEG monomers (∼794/2 = 397), so the actual number = 397 * 0.167 = ∼ 66 α-CD per chain d. The number of α-CD per PEG chain with full coverage is half the number of PEG monomers (∼794/2 = 397), so the actual number = 397 * 0.167 = ∼ 66 α-CD per chain 2.Validation of PR-alkyne functionality is done via 1H-NMR spectroscopy (Fig. 3C)2.1.To determine the alkyne functionality, the integration of the 6 Ha α-CD protons was normalized. The alkyne peak at 4.30 thus represented the number of alkyne groups per ring. For hydroxypropyl functionality, the methyl He peak integration was divided by three to calculate the number of hydroxypropyl groups incorporated per ring. In our experience, ∼1-2 alkyne per ring and >3 hydroxypropyl groups per ring yielded the best results for subsequent reactions, though these can be modified depending on the desired final functionality. In the representative example shown (Fig. 3C), the α-CD rings were functionalized with 2.1 alkyne and ∼3.9 hydroxypropyl groups per ring. Given a ring coverage of 10.8% and a theoretical maximum of 397 rings per PR chain for 100% coverage (Table 1), each PR contains ∼43 rings. Thus, this batch of polymer contains approximately 90 alkyne groups per macromer.2.2.PR-Alkyne: 1H-NMR (500 MHz, DMSO) δ: ∼5.35-5.00 (6 Ha), 4.30 (1 Hb), 4.2-3.3 (36 Hc + 74 *Hd), 1.20 (24 *He).2.3.*Values vary between batches of polymer depending on glycidyl propargyl ether and propylene oxide incorporation. Validation of PR-alkyne functionality is done via 1H-NMR spectroscopy (Fig. 3C)2.1.To determine the alkyne functionality, the integration of the 6 Ha α-CD protons was normalized. The alkyne peak at 4.30 thus represented the number of alkyne groups per ring. For hydroxypropyl functionality, the methyl He peak integration was divided by three to calculate the number of hydroxypropyl groups incorporated per ring. In our experience, ∼1-2 alkyne per ring and >3 hydroxypropyl groups per ring yielded the best results for subsequent reactions, though these can be modified depending on the desired final functionality. In the representative example shown (Fig. 3C), the α-CD rings were functionalized with 2.1 alkyne and ∼3.9 hydroxypropyl groups per ring. Given a ring coverage of 10.8% and a theoretical maximum of 397 rings per PR chain for 100% coverage (Table 1), each PR contains ∼43 rings. Thus, this batch of polymer contains approximately 90 alkyne groups per macromer.2.2.PR-Alkyne: 1H-NMR (500 MHz, DMSO) δ: ∼5.35-5.00 (6 Ha), 4.30 (1 Hb), 4.2-3.3 (36 Hc + 74 *Hd), 1.20 (24 *He).2.3.*Values vary between batches of polymer depending on glycidyl propargyl ether and propylene oxide incorporation. 2.1.To determine the alkyne functionality, the integration of the 6 Ha α-CD protons was normalized. The alkyne peak at 4.30 thus represented the number of alkyne groups per ring. For hydroxypropyl functionality, the methyl He peak integration was divided by three to calculate the number of hydroxypropyl groups incorporated per ring. In our experience, ∼1-2 alkyne per ring and >3 hydroxypropyl groups per ring yielded the best results for subsequent reactions, though these can be modified depending on the desired final functionality. In the representative example shown (Fig. 3C), the α-CD rings were functionalized with 2.1 alkyne and ∼3.9 hydroxypropyl groups per ring. Given a ring coverage of 10.8% and a theoretical maximum of 397 rings per PR chain for 100% coverage (Table 1), each PR contains ∼43 rings. Thus, this batch of polymer contains approximately 90 alkyne groups per macromer. To determine the alkyne functionality, the integration of the 6 Ha α-CD protons was normalized. The alkyne peak at 4.30 thus represented the number of alkyne groups per ring. For hydroxypropyl functionality, the methyl He peak integration was divided by three to calculate the number of hydroxypropyl groups incorporated per ring. In our experience, ∼1-2 alkyne per ring and >3 hydroxypropyl groups per ring yielded the best results for subsequent reactions, though these can be modified depending on the desired final functionality. In the representative example shown (Fig. 3C), the α-CD rings were functionalized with 2.1 alkyne and ∼3.9 hydroxypropyl groups per ring. Given a ring coverage of 10.8% and a theoretical maximum of 397 rings per PR chain for 100% coverage (Table 1), each PR contains ∼43 rings. Thus, this batch of polymer contains approximately 90 alkyne groups per macromer. 2.2.PR-Alkyne: 1H-NMR (500 MHz, DMSO) δ: ∼5.35-5.00 (6 Ha), 4.30 (1 Hb), 4.2-3.3 (36 Hc + 74 *Hd), 1.20 (24 *He). PR-Alkyne: 1H-NMR (500 MHz, DMSO) δ: ∼5.35-5.00 (6 Ha), 4.30 (1 Hb), 4.2-3.3 (36 Hc + 74 *Hd), 1.20 (24 *He). 2.3.*Values vary between batches of polymer depending on glycidyl propargyl ether and propylene oxide incorporation. *Values vary between batches of polymer depending on glycidyl propargyl ether and propylene oxide incorporation. 3.Validation of final PR-Hyd functionality and boc-deprotection are confirmed via 1H-NMR spectroscopy (Fig. 4C-G)3.1.The 6 Hb α-CD protons were again used for normalization. The peak at 8.09 ppm corresponded to the triazole proton (Ha) that appeared after CuAAC crosslinking and was therefore used to quantify the number of hydrazine molecules per α-CD ring.3.2.Boc-protected PR-Hyd: 1H-NMR (500 MHz, DMSO) δ: 8.09 (1 Ha), ∼5.10-4.60 (6 Hb), ∼4.00-3.02 (36 Hc + 42 *Hd), 1.40 (27 He), 1.01 (12 *Hf).3.3.PR-Hyd: 1H-NMR (500 MHz, DMSO) δ: 8.09 (1 Ha), ∼5.35-5.00 (6 Hb), ∼4.20-3.30 (36 Hc + 76 *Hd), 1.20 (12 *He).3.4.In the representative spectrum shown (Fig. 4D), the polymer exhibited an α-CD coverage of 10.5% with a functionality of 0.4 hydrazine per ring. This equates to approximately 42 rings and 16 hydrazine functional groups per macromer. Notably, values marked with asterisks vary between synthesis batches and should be quantified for each new batch of polymer. Validation of final PR-Hyd functionality and boc-deprotection are confirmed via 1H-NMR spectroscopy (Fig. 4C-G)3.1.The 6 Hb α-CD protons were again used for normalization. The peak at 8.09 ppm corresponded to the triazole proton (Ha) that appeared after CuAAC crosslinking and was therefore used to quantify the number of hydrazine molecules per α-CD ring.3.2.Boc-protected PR-Hyd: 1H-NMR (500 MHz, DMSO) δ: 8.09 (1 Ha), ∼5.10-4.60 (6 Hb), ∼4.00-3.02 (36 Hc + 42 *Hd), 1.40 (27 He), 1.01 (12 *Hf).3.3.PR-Hyd: 1H-NMR (500 MHz, DMSO) δ: 8.09 (1 Ha), ∼5.35-5.00 (6 Hb), ∼4.20-3.30 (36 Hc + 76 *Hd), 1.20 (12 *He).3.4.In the representative spectrum shown (Fig. 4D), the polymer exhibited an α-CD coverage of 10.5% with a functionality of 0.4 hydrazine per ring. This equates to approximately 42 rings and 16 hydrazine functional groups per macromer. Notably, values marked with asterisks vary between synthesis batches and should be quantified for each new batch of polymer. 3.1.The 6 Hb α-CD protons were again used for normalization. The peak at 8.09 ppm corresponded to the triazole proton (Ha) that appeared after CuAAC crosslinking and was therefore used to quantify the number of hydrazine molecules per α-CD ring. The 6 Hb α-CD protons were again used for normalization. The peak at 8.09 ppm corresponded to the triazole proton (Ha) that appeared after CuAAC crosslinking and was therefore used to quantify the number of hydrazine molecules per α-CD ring. 3.2.Boc-protected PR-Hyd: 1H-NMR (500 MHz, DMSO) δ: 8.09 (1 Ha), ∼5.10-4.60 (6 Hb), ∼4.00-3.02 (36 Hc + 42 *Hd), 1.40 (27 He), 1.01 (12 *Hf). Boc-protected PR-Hyd: 1H-NMR (500 MHz, DMSO) δ: 8.09 (1 Ha), ∼5.10-4.60 (6 Hb), ∼4.00-3.02 (36 Hc + 42 *Hd), 1.40 (27 He), 1.01 (12 *Hf). 3.3.PR-Hyd: 1H-NMR (500 MHz, DMSO) δ: 8.09 (1 Ha), ∼5.35-5.00 (6 Hb), ∼4.20-3.30 (36 Hc + 76 *Hd), 1.20 (12 *He). PR-Hyd: 1H-NMR (500 MHz, DMSO) δ: 8.09 (1 Ha), ∼5.35-5.00 (6 Hb), ∼4.20-3.30 (36 Hc + 76 *Hd), 1.20 (12 *He). 3.4.In the representative spectrum shown (Fig. 4D), the polymer exhibited an α-CD coverage of 10.5% with a functionality of 0.4 hydrazine per ring. This equates to approximately 42 rings and 16 hydrazine functional groups per macromer. Notably, values marked with asterisks vary between synthesis batches and should be quantified for each new batch of polymer. In the representative spectrum shown (Fig. 4D), the polymer exhibited an α-CD coverage of 10.5% with a functionality of 0.4 hydrazine per ring. This equates to approximately 42 rings and 16 hydrazine functional groups per macromer. Notably, values marked with asterisks vary between synthesis batches and should be quantified for each new batch of polymer. Limitations Not applicable. Ethics statements Not applicable. CRediT authorship contribution statement Sarah J. Loveland: Conceptualization, Formal analysis, Funding acquisition, Investigation, Methodology, Validation, Visualization, Writing – original draft, Writing – review & editing, Supervision. Xinming Tong: Conceptualization, Funding acquisition, Investigation, Methodology, Validation, Writing – review & editing. Hung-Pang Lee: Methodology, Validation, Writing – review & editing. Christine L. Zhou: Methodology, Validation, Writing – review & editing. Fan Yang: Conceptualization, Funding acquisition, Project administration, Resources, Supervision, Writing – original draft, Writing – review & editing. Declaration of competing interest The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.