Enhancing the energy storage capacity of a symmetric supercapacitor employing α-Cu2P2O7 produced by a template-based co-precipitation approach Authors: Jay B. Patel, Karan S. Modi, Pruthvi Patel, Dharti Patel, Vanaraj Solanki, Bhavin Patel, Mitesh H. Patel Published: 2026 ABSTRACT Pyrophosphates have acquired considerable attention as a potential electrode material in energy storage devices owing to their strong covalent P–O bonds, which ensure structural stability, high electrochemical activity, and efficient ion migration. In this contribution, we synthesized copper pyrophosphate (Cu2P2O7) by using a simple co-precipitation method followed by calcination at 500 °C for 30 minutes. The monoclinic structure of the material with space group C12/c1 was confirmed by powder X-ray diffraction. The Cu2P2O7 bonds were confirmed using Raman spectroscopy, while Fourier transform infrared spectroscopy confirmed the bending vibration of P–O–P and P–O bonds. X-ray Photoelectron Spectroscopy validates the +2-oxidation state of copper and the +5-oxidation state of phosphorus. Field emission scanning electron microscope revealed that the interconnected porous morphology with a rough surface of the material provides abundant active sites for ion movements and facilitates electrolyte penetration. The symmetric supercapacitor device of Cu2P2O7 possesses an excellent specific capacity of 225 F g−1 with a power density and energy density of 3200 W kg−1 and 80 Wh/kg at a current density of 1 A g−1, respectively. The symmetric device retains about 90% of its initial capacity after 10 000 cycles at a current density of 1.5 A g−1. The symmetric device is capable to illuminate a single 3 V red light emitting diode continuously for 1 minute and 27 seconds. The electrochemical findings endorse the viability of Cu2P2O7 as a suitable electrode material for long-term energy storage applications. Introduction Given the limited availability of fossil fuels, research into energy storage devices is crucial for identifying alternatives that can prevent environmental deterioration while being both functional and economically viable to satisfy future energy requirements. In the context of energy generation and storage, batteries, solar cells and supercapacitors (SCs) are the three possible and effective options. Among them, SCs have garnered more attention due to their high-power density, long life cycle, low cost, and environmental friendliness. Additionally, their charge storage capacities can be modified, rendering them compatible with Li-ion batteries. These unique attributes making them ultimate choice for electric vehicles, portable devices, and some biomedical apparatus.1–6 The electrochemical characteristics, including energy density, power density, rate capability, and cycle stability, are essential metrics dependent on electrode materials. Currently, carbon,7–10 graphene,11–13 mono-metallic oxides,14 metal sulphides,15–18 conducting polymers,19–23 bi metallic oxides,24,25 metal hydroxides26,27 and Mxene28,29 have been studied as an electrode material owing to its high surface area, short diffusion length and excellent cyclic stability. The synthesis method employed to produce these electrode materials was intricate and time-consuming, rendering it impractical for industrial usage. The industrial revolution of electrode materials necessitates the advancement of economical, straightforward, and eco-friendly synthesis processes that not only lower expenses but also ensure an unpolluted environment. Metal pyrophosphates (M2P2O7, M; Cu, Ni, Co, Zn, Fe) have recently received a lot of interest among the researchers because of their extraordinary electrochemical properties, enabling their utilization in various applications including; energy storage, energy conversion, catalysis.30–33 Their distinctive attributes, including a layered structure, excellent reversibility, high electrical conductivity, admirable corrosion resistance, and redox stability, render them appropriate for use in energy storage devices, presenting them as competitive alternatives to conventional electrode materials. Researchers have conducted sustainable effort to investigate the electrochemical characteristics of pyrophosphates by selecting various combinations of metals with phosphates and pyrophosphates including; nickel,34 cobalt,35 copper,36 ferrous,37 and nickel-cobalt38 with various morphologies. Among various combinations, the combination of copper with pyrophosphate is unique and exceptional owing to its low-cost, non-toxic material, and higher intrinsic conductivity, which facilitates quicker electron transit, positioning it as a viable alternative to conventional nickel or cobalt phosphates.39,40 According to literature, Glaser et al.41 prepared Cu2P2O7 by flux method to identify the structure and phase transition of Cu2P2O7. From this study they have concluded that Cu2P2O7 exhibits two stable crystalline phases: α- Cu2P2O7 at low temperature and β- Cu2P2O7 at higher temperature. To understand enthalpy and thermal behavior of Cu2P2O7 Le et al.42 employed a solution based acidification approach to prepare α-Cu2P2O7 from copper sulfate and tetra sodium pyrophosphate. The blue crystals were collected and turned into pellets for calcination at 600 °C in air for three days. Karaphun et al.43 investigated the influence of calcination temperature on the physical and electrochemical characteristics of Cu2P2O7 prepared by hydrothermal method. From this study, they have concluded that Cu2P2O7 powder heated to 550 °C has the maximum specific capacitance of 297.521 F g−1 at 1 A g−1, as well as strong cycling stability even after 1000 cycles (94.04% retention). Agarwal et al.43 used the Successive ionic layer adsorption and reaction (SILAR) method for the preparation of ultrathin nano flakes of Cu2P2O7 directly on stainless steel electrode for SCs application. The symmetric supercapacitor device fabricated from Cu2P2O7 nanoflakes exhibit a capacitance of 102.5 F g−1 at a current density of 5 A g−1, with an energy density of 11.54 Wh/kg and a power density of 2760 W kg−1. Likewise, Lee et al.45 developed a Cu2P2O7/carbon nanotube composite cathode for sodium battery conversion. They have prepared Cu2P2O7 using wet ball-milling process followed by calcination at 850 °C for 10 h. The Cu2P2O7/carbon nanotube composite cathode material was prepared by mixing 1 wt% carbon nanotube with Cu2P2O7 using high energy ball milling at 100 rpm for 12 h. The resulting cathode has a high capacity of 355 mA h g−1, an average operation voltage of 2.4 V (versus Na+/Na), and retains 75% of its initial capacity after 300 cycles at 360 mAg−1. In different approach, Mangate et al.46 produced one dimensional nanofiber of Cu2P2O7 by using straightforward polymer-based electro spinning method followed by calcination for asymmetric supercapacitor application. The asymmetric device was constructed utilizing Cu2P2O7 nanofibers as the cathode and carbon fiber as the anode material, demonstrating a specific capacitance of 143.73 F g−1 at a current density of 0.4 A g−1. The energy density of the device was measured at 57.69 Wh/kg, while the power density reached 1104.7 W kg−1, retaining 92.9% of its capacity after 2000 cycles. As per the literature, the synthesis of pyrophosphate has been described by several processing tactics, including the Flux method,41 hydrothermal techniques,43 acidification,42 electrospinning processes,46 Hydrogen bonding,47,48 and catalytic method.49 Further, the polymer mediated co-precipitation method for the synthesis of α-Cu2P2O7 for symmetric SCs application not been reported yet. Hence, present study focuses on a cost-effective Polyvinyl pyrrolidone (PVP) mediated co-precipitation approach followed by calcination to prepare α-Cu2P2O7 and investigate its electrochemical characteristics for future symmetric SCs devices. Materials and methods Chemicals and materials For the synthesis of Cu2P2O7, PVP (M.W.: 40 000), Cu(NO3)2·6H2O (copper nitrate hexahydrate), Na4P2O7 (Tetrasodium pyrophosphate), polyvinylidene fluoride (PVDF), potassium hydroxide (KOH), Ns-Methyl-2-pyrrolidone (NMP), cellulose filter paper was procured from Loba Chemie Pvt, Ltd. Multi-Walled Carbon Nano Tubes (MWCNT) and carbon cloth werse obtained from Technistro Industries, India. CR-2032 type coin cell was procured from Bat-sol Equipment and Technology Pvt Ltd, India. All these chemicals were used as received without further purification. Experimental section Synthesis of Cu2P2O7 The template-based synthesis of Cu2P2O7 was conducted by addition of 0.3 g of PVP with a stoichiometric mass of Cu(NO3)2·6H2O, both dissolved in 25 ml of Milli-Q water, alongside Na4P2O7, which was dissolved separately in 25 ml of MilliQ water. To get the precipitate, add the Na4P2O7 solution steadily to the previously described solution while stirring constantly. The resultant precipitate had been separated using centrifugation at 6000 rpm and subsequently dried in an oven at 50 °C for one hour. The resultant material was finally calcined at 500 °C in a muffle furnace for 30 minutes, with a heating rate of 1.66 °C per minute, to obtain the final Cu2P2O7 (Scheme 1). Experimental procedure for the synthesis of Cu2P2O7. Fabrication of electrode The electrode was fabricated by mechanically grinding the mixture of Cu2P2O7 as an active material, carbon black as a conducting agent, and PVDF as a binder at a weight ratio of 80 : 15 : 5, with a few drops of NMP as a solvent, in a mortar and pestle until a homogeneous slurry was achieved. This slurry was carefully coated on clean nickel foam and was allowed to dry for 10 hours at 60 °C to eliminate the remaining NMP solvent and ensure adherence. Electrode setup for symmetric supercapacitor A symmetric supercapacitor (SCs) device was constructed utilizing a CR2032-type coin cell, with both the positive and negative electrodes composed of the identical active material, Cu2P2O7, and applied onto a stainless-steel current collector, maintaining comparable weights. The electrodes were positioned between cellulose paper that had been saturated with 6 M KOH, which acted as the electrolyte. Characterization The material's structure was analyzed by X-ray diffraction (XRD) (Bruker, D2 PHASER) using Ni-filtered CuKα radiation (λ = 1.5418 Å), with a 2θ range of 10° to 70°. Rietveld refinement on the experimental data was performed using the FULLPROF package. Thermo Fisher Scientific (Phenom Pharos G2) was used for Field emission scanning electron microscope (FE-SEM) and Energy Dispersive X-ray spectroscopy (EDX) to evaluate the morphology and elemental analysis of the prepared sample. High resolution transmission electron (HR-TEM) by JEOL JEM 2100+ instruments was used to analyzed the internal structure of the material. Raman Spectroscopy was performed on an iRaman plus equipped with 532 nm diode laser, with the wavenumber range of 240 to 1200 cm−1. The Fourier transform infrared spectroscopy (FTIR) was performed on a SHIMADZU IR-Spirit-X spectrometer in the range of 400 to 2800 cm−1. The X-ray photoelectron spectroscopy (XPS) was performed using Nexsa G2 instrument by Thermo Scientific. The surface area and porosity were determined through Brunner-Emmet-Teller (BET) analysis utilizing a Quantachrome AUTOSORB iQ made by Anton Paar Instruments. The electrochemical measurements of Cu2P2O7 material were determined using the Gamry Instruments 1010-E electrochemical workstation. The electrochemical behaviour of Cu2P2O7 was carried out with respect to Hg/HgO as a reference electrode and Pt Spring serving as the counter electrode in a 6 M KOH aq. electrolyte. Results and discussion X-ray diffraction The phase composition and crystal structure of the material were analysed with the help of an XRD instrument. Fig. 1(a) exhibits the XRD pattern and Rietveld refinement for the α-Cu2P2O7 sample. Rietveld refinement was performed to study the crystal structure of the α-Cu2P2O7 sample; the crystallographic instrument file (CIF) for the same is included in the supplementary information. In the refining phase, the profile form was defined by the pseudo-Voigt function, while the background was linearly interpolated between specified locations, incorporating height modifications. All other parameters, including the scale factor, zero correction, background, mixing parameters, lattice parameters, and atomic coordinates, were similarly adjusted. It can be observed that the experimental data (navy colored) aligns well with the calculated data (black colored), as the difference between the experimental and calculated patterns was attempted to be minimized (purple colored). The dark vertical red lines indicate the Bragg position of the synthesized α-Cu2P2O7 material ICDD card no. 21-0299. The refining findings indicated a χ2 value of 1.67. Table 1 enumerates the crystallographic information regarding the crystal plane and atomic parameters of the refined data. Additionally, the main five peaks at 28.32°, 30.20°, 30.48°, 35.40°, and 35.94° are accurately attributed to the (2̄02), (022), (112), (220), and (130) planes, respectively.36,43,44 The XRD pattern supports a monoclinic structure with the space group C12/c1, which is known as the alpha (α) phase of Cu2P2O7.42,50 The lattice parameters obtained from refinement are, a = 6.844 Å, b = 8.117 Å, and c = 9.139 Å with α = γ = 90° and β = 109.21°42,50 which are comparable with the previously reported data.36,44,45 (a) X-ray diffractogram and (b) tetrahedral structure of material, where the green, blue, and red colours represent Cu, P, & O atoms of α-Cu2P2O7 material. Table 1Detail Rietveld refinement data of α-Cu2P2O7AtomMultiplicityWyckoff site X Y Z B iso OccupancyCu88f−0.007800.312280.508050.340111.00000P88f0.20039−0.003830.206320.780271.00000O144e0.000000.045570.250000.538281.00000O288f0.380420.010150.351550.243731.00000O388f0.168240.150640.111620.853401.00000O488f0.21913−0.150360.11964−1.125901.00000 Detail Rietveld refinement data of α-Cu2P2O7 The phase composition and crystal structure of the material were examined using Fig. 1(b). The crystal structure of α-Cu2P2O7 was generated using VESTA software taking values from Table 1. This software provided an accurate and detailed depiction of the α-Cu2P2O7 structure and atomic arrangement. This crystal structure has an open geometry that defines the arrangement of atoms linked by oxygen atoms. It depicts a tetrahedral configuration of oxygen atoms that includes copper and phosphorus atoms, as illustrated in Fig. 1(b). Fourier transform infrared spectroscopy and Raman spectroscopy The FTIR was used alongside Raman spectra to get additional information regarding the vibrational mode and phase identification of the synthesized material. The FTIR spectrum, spanning from 2800 cm−1 to 400 cm−1, was illustrated in Fig. 2(a). The peak attributed at 517 cm−1 was demonstrated as an asymmetric bending vibration of the P–O bonds, whereas the peak located at 556 cm−1 represents P–O deformation.46 Moreover, the stretching vibration of P Created by potrace 1.16, written by Peter Selinger 2001-2019 O was observed at 723 cm−143 while the PO4−3 anion was noticed at a wavenumber of 767 cm−1.4 Furthermore, the asymmetric vibration mode of the P–O–P bond was attributed at 906 cm−146 Moreover, the peak located at 956 cm−1 was responsible for PO stretching vibration.43 The symmetric stretching of the PO3 group was associated with 1078 cm−146 The absorption band identified at 1635 cm−1 was ascribed to the stretching vibration of the H–O–H of the prepared Cu2P2O7 material.43 (a) FTIR spectrum and (b) Raman spectrum of Cu2P2O7. The phase identification and distinctive stretching/bending vibrations of Cu2P2O7 were analysed using Raman spectroscopy. The Raman spectra of Cu2P2O7 show the signal at 1144 cm−1 was associated with υas (PO3), while the spikes at 1080 cm−1 & 1051 cm−1 were identified as υs(PO3), respectively. Likewise, the observed bands at 740 cm−1, 650 cm−1, and 406 cm−1 were concomitant with a symmetric vibration of the P–O–P bridge. Furthermore, the peaks at 544 cm−1 corresponded to the asymmetric bending vibration of the P–O bond, whereas the vibration at 358 cm−1 and 310 cm−1 correlate with the PO3 and P–O–P bonds.50 Moreover, the distinctive peaks at 1144 cm−1 and 1051 cm−1 in the Raman spectra corroborate the production of α-Cu2P2O7, which aligns with the XRD results. Field emission scanning electron microscope images The morphological assessment serves as a practical approach aimed at substantially improving the overall effectiveness of materials for electrochemical applications. Fig. 3 displays FE-SEM images of the Cu2P2O7 material, emphasizing its surface structure at various resolution. Fig. 3(a) shows irregular polygonal-shaped structures in the form of thin nanoflakes. Upon higher resolution (Fig. 3(b)), it can be observed that the structures are nano-size and have a rough surface area due to a higher calcination temperature. The interconnected morphology of developed α-Cu2P2O7 forms a porous network with a rough surface, which establishes a clear structure–activity relationship. The high surface roughness maximizes electrochemically active sites, the porous architecture facilitates rapid ion diffusion and electrolyte penetration, and the interconnected framework ensures efficient electron mobilization.51 (a and b) FE-SEM images of Cu2P2O7 material. Energy dispersive X-ray spectroscopy An elemental composition of the Cu2P2O7 was performed using EDX. The EDX spectrum of Cu2P2O7, illustrated in Fig. 4(a). Fig. 4 (b–e) represent the elemental mapping which verifies the existence of copper (Cu), phosphorus (P), and oxygen (O) atoms ratio. EDX analysis reveals the atomic percentage of Cu, P, and O as 13.4%, 19.8% and 66.6% respectively, corresponding to an atomic ratio of Cu : P : O = 1.35 : 2 : 6.76, which is in close agreement with the theoretical stoichiometry of α-Cu2P2O7 (Cu : P : O = 2 : 2 : 7), confirming the successful formation of Cu2P2O7. Furthermore, there are no other element peaks observed in the spectrum, further substantiating the purity of the α-Cu2P2O7. (a) EDX spectrum and (b–e) elemental mapping of α-Cu2P2O7. High-resolution transmission electron microscope The internal structure of as prepared material was meticulously investigated through HR-TEM analysis. Fig. 5(a) displays the low-magnification TEM illustration, which shows polygonal-shaped particles having an interconnected porous structure, in accordance with the morphology identified in FE-SEM analysis. The statistical analysis of particle dimension from TEM image (Fig. 5(b)) reveals an average particle size of 44.19 nm, underscoring the nanoscale characteristics of the as synthesized material, which is likely to improve the electrode–electrolyte contact area. Fig. 5(c) shows a higher resolution TEM picture that displays the granular surface roughness of individual particles, enabling several active sites for ion adsorption and diffusion. Fig. 5(d) High resolution transmission electron microscopy (HR-TEM) image of material, with targeted area enlarged in Fig. 5(e). Distinctly defined and very regular lattice fringes are visible throughout the particle internal structure, affirming the elevated crystallinity of the synthesized material. The interplanar spacing of d = 0.32 nm aligns with the (200) crystal plane of α-Cu2P2O7, corroborating the predicted d-spacing derived from the XRD data (ICDD card no.: 21-0299). Fig. 5(f) further emphasizes the pronounced contrast and well-organized lattice tresses, therefore confirming the material's homogeneous crystalline structure. The selected area electron diffraction (SAED) pattern (Fig. 5(g)) displays three distinct concentric diffraction rings corresponding to the (002), (200), and (2̄02) planes of α-Cu2P2O7, thereby supporting the polycrystalline character of the as prepared material and aligning with the monoclinic crystal structure determination by XRD analysis. The HR-TEM and SAED investigations provides direct atomic scale confirmation of the remarkable crystallinity and phase purity of α-Cu2P2O7, therefore demonstrating a definitive structure–activity link between the crystalline nanostructure and the reported electrochemical performance.36,44,46 (a) Overall morphology (b) average particle size histogram (c) particle shape (d) HR-TEM region (e) inter layer d-spacing image (f) enlarge image of figure (e) (g) SAED pattern of α-Cu2P2O7. X-ray photoelectron spectroscopy The XPS analysis was conducted to examine the oxidation states of Cu, P, and O atoms in the α-Cu2P2O7 material within the energy range of 0 to 1200 eV. Fig. 6(a) illustrates the XPS survey scan, which shows the group of signals representing Cu2p and P2p as well as O1s, confirming the availability of Cu, P, and O atoms in α-Cu2P2O7 material, including the background peak with C 1s. In addition, the peak at 569.98 eV corresponds to the Cu LMM band, while another peak of the O KLL band appears at 978 eV. Meanwhile, the binding energy of 78 eV is correlated with the Cu3p band. Moreover, Fig. 6(b) displays the narrow spectrum of Cu2p, indicating two spin–orbit peaks at 956.6 eV and 936.5 eV are aligned with Cu2p1/2 and Cu2p3/2, whereas the two satellite signals appear at binding energies of 963.8 eV and 944.1 eV, respectively. Furthermore, the P2p binding energy observed at 133.4 eV confirms the presence of phosphorus with pentavalent state (P5+). In the same vein, the deconvolved high-resolution O 1 s signal, Fig. 6(d), is identified by two significant peaks: one at 531.5 eV, linked to O atoms in Cu–O–P bonds, and the other at 533 eV, ascribed to surface-adsorbed O2 bonds.44,46 The results unequivocally show the oxidation state of the α-Cu2P2O7 molecule. XPS spectra of copper pyrophosphate material: (a) survey scan, (b) Cu 2p, (c) P 2p, and (d) O 1s of α-Cu2P2O7 material. The XPS survey spectrum affirms the existence of Cu, P, and O in prepared α-Cu2P2O7 material. As per Table 2, the quantitative assessment of the XPS survey scan identifies atomic percentage of Cu at 12.6%, P at 18.2% and O at 69.1%. The P2p atomic percentage closely aligned with the EDX derived value and the estimated stoichiometry of synthesized material. The minor deviation in copper (Cu) atomic percentage between EDX and XPS is ascribed to the intrinsically surface-sensitive characteristic of XPS, where surface phosphate enrichment and the intricate multi-dimensional structure of Cu2+ in survey mode may influence quantitative precision. Table 2Comparison table for XPS atomic% and EDX atomic% data of α-Cu2P2O7ElementXPS (%)EDX (%)Cu12.613.4P18.219.8O69.166.6 Comparison table for XPS atomic% and EDX atomic% data of α-Cu2P2O7 BET analysis The specific surface area of Cu2P2O7 material was measured using the BET method, while pore size distribution was analyzed using the Brunauer-Joyner-Halenda model. In Fig. 7(a), a characteristic of type IV isotherms was identified52 in the nitrogen adsorption–desorption isotherm of the α-Cu2P2O7 compound. The specific surface area (SSA) of the synthesized α-Cu2P2O7 was accurately measured at 10.038 m2 g−1. Additionally, mesopores with diameters between 15 nm and 88 nm have been detected in the analysis of the pore-size distribution displayed in Fig. 7(b). The almost parallel adsorption and desorption paths indicate a very homogeneous pore size distribution. The SSA of α-Cu2P2O7 particles gives a significant number of active sites for ion diffusion. (a) Nitrogen adsorption and desorption isotherm and (b) pore size distribution curve of α-Cu2P2O7 powder. Electrochemical exploration of synthesized α-Cu2P2O7 material Three-electrode measurement The electrochemical evaluation of the synthesized α-Cu2P2O7 electrode was conducted via CV across various potential windows of 0 to 0.5 V, 0.6 V, and 0.7 V at 20 mV s−1 depicted in Fig. S(4(a)); it can be observed that beyond 0.6 V a clear polarization effect is observed restricted the capacity of the α-Cu2P2O7 electrode. Thus, the effective potential range is selected between 0 and 0.6 V. Fig. 8(a) depicts CV with scan rates ranging from 10 to 100 mV s−1. The α-Cu2P2O7 electrode displays a quasi-rectangular CV curve with peaks at 0.15 V, suggesting pseudo-capacitance behavior. Furthermore, the large anodic and cathodic redox peaks indicate quasi-reversible electron transport at the electrode–electrolyte interface during the faradaic redox phenomenon, resulting in Cu ion oxidation state switching.43 The area under the CV curve expands with the increase in scan rate, which signifies a direct relation between scan rate and voltametric current. The shape of the curve remains unchanged even when the scan rate is increased, signifying a reversible charge transfer reaction in conjunction with surface adsorption. There was an absence of gas genesis on the electrodes, and no change in electrolyte color was seen during CV testing at different scans. This signifies that the synthesized mesoporous α-Cu2P2O7 electrode material exhibits improved stability over the 0 V to 0.6 V potential range. (a) Cyclic voltammogram (CV), (b) galvanic charge–discharge cycles (GCD), (c) specific capacitance at various current densities, (d) capacity retention and coulombic efficiency measurement for 5000 charge–discharge cycles (e) electrochemical impedance spectroscopy (EIS) of before stability and fitted (f) equivalent circuit of α-Cu2P2O7. Eqn (1) and (2) pertain to the reaction process of the α-Cu2P2O7 electrode:1[Cu2P2O7]Surface + K+ + e− [K+Cu2P2O7]Surface2[K+Cu2P2O7]Surface [Cu2P2O7]Surface + K+ + e− This reaction process suggests that electrolyte cations (K+) adsorb onto the electrode's surface, forming a thin layer between the electrode electrolyte interface (eqn (1)). These cations then diffuse back into the electrolyte solution during discharging, thereby releasing the energy (eqn (2)).53 Fig. 8(b) illustrates the GCD profile of the material throughout the voltage band from 0 V to 0.6 V. Each curve displays a subtly deformed triangular form that emphasizes fast surface redox reactions. The specific capacitance was determined by employing eqn (3);53,543where, Current density denoted by I/m, m is contingent upon the active mass (m). Δt represents the cumulative discharge duration, and ΔV represents the complete potential range. The specific capacitance values of the α-Cu2P2O7 electrode are 667, 630, 607, 587, 555, and 533 F g−1 at current densities of 5, 6, 7, 8, 9, and 10 A g−1, respectively. Fig. 8(c) depicts the capacitance vs. current density graph, indicating a decline in capacitance as the applied current density increases. This is due to the limited time for ions to interact with the electrode surface as the current density increases. The specific capacitance in the three-electrode configuration is relatively superior compared to the previously published α-Cu2P2O7 material synthesised by various methods.36,43,44,55 Furthermore, the energy density and power density were calculated from GCD curves at various current densities using eqn (4) and (5):53,5645where, E and P denoted as energy density and power density, Specific capacitance is denoted as Csp, Voltage window, denoted by ΔV, The discharge time is represented by Δt. The determined energy density and power density values of the electrode are 45 Wh kg−1 at 2041 W kg−1, 43 Wh kg−1 at 2450 W kg−1, 41 Wh kg−1 at 2858 W kg−1, 40 Wh kg−1 at 3266 W kg−1, and 38 Wh kg−1 at 3675 W kg−1.67where, td and tc are the present discharge time and charging time, respectively. Electrode stability was analysed for continuous 5000 charge–discharge cycles with its corresponding coulombic efficiency at a current density of 12 A g−1 as shown in Fig. 8(d). The specific capacitance retention and coulombic efficiency were calculated by eqn (6) and (7). The electrode material demonstrates a robust capacity retention of 90% from its initial capacity and a superior coulombic efficiency of 80%, thereby affirming the exceptional long-term cycling stability of the synthesized α-Cu2P2O7 material. The electrode material exhibits superior stability performance when compared with previously reported α-Cu2P2O7 material's data.4,36,43,44,46 The EIS technique was employed to determine the charge transfer characteristics of the α-Cu2P2O7 electrode. The Nyquist plot, portrayed in Fig. 8(e), shows the changes observed before and after 5000 consecutive cycles of the α-Cu2P2O7 electrode, covering a frequency range from 0.1 Hz to 1 MHz. The corresponding fitted circuit is shown in Fig. 8(f). The observed data and fitted data are separated into two regions: (i) a semicircle represents the high-frequency zone, and (ii) a linear line represents the low-frequency region. In addition, Table 3 displays the values obtained from the fitted data. Where series resistance (Rs) is the total resistance provided by the electrode, electrolyte, and current collector. Charge-transfer resistance (Rct) is the resistance that ions face at the electrode/electrolyte interface. Double-layer capacitance (CPEDL) results from the separation of ionic charges at the electrode–electrolyte interface, and the Warburg element (W) depicts the diffusion of ions into the electrode and vice versa. As the cycle number increased from 1 to 5000, the Rs value also increased from 8.6464 Ω to 9.12 Ω. This demonstrates that capacity declines during an extended charge–discharge cycle as a result of higher resistance. The observed Rct value decreases from 0.5921 Ω to 0.1719 Ω, the cause for the decreasing value of Rct is the rapid flow of ions within the device, which reduces the effective capacitance. The CPEDL value increases due to the accumulation of opposite charges across the electrode–electrolyte interface. Furthermore, the Warburg impedance has increased because the ion diffusion rate is more impeded.53,56,57 As the number of charge–discharge cycles grows, so does the resistance encountered by the ions, reducing the device's overall performance. Table 3Fitted values of circuit elements for the 1st and 5000th cycles for three electrode measurementα-Cu2P2O7 R s (Ω) R CT (Ω)CPEDL (S sn) W (Ω · s−1/2)1st8.64640.59212.508 × 10−30.15385000th9.120.171930.13 × 10−30.2426 Fitted values of circuit elements for the 1st and 5000th cycles for three electrode measurement Symmetric supercapacitor device The schematic layout of the coin cell (Scheme 2) shows its major components grouped in series, including the cap and can, which are used to firmly close the cell. A spring is used to maintain pressure and ensure contact between the two electrodes. The stainless-steel plates serve as a current collector that are uniformly covered with a slurry of electrode material, forming both an anode and cathode. The separator was inserted between the electrodes to allow ionic flow while avoiding short connections. This sort of coin cell configuration offers mechanical stability, ionic transport assistance, and excellent electrochemical performance. Schematic diagram of symmetric coin cell configuration. Fig. 9(a) shows the CV curve of prepared α-Cu2P2O7 at scan rates ranging from 10 mV s−1 to 100 mV s−1 within a potential window of 0 to 1.6 V. The quasi-rectangular shape of the CV with a redox peak is observed during the analysis; this characteristic of the CV signifies that the material exhibits pseudocapacitive behaviour and ion intercalation and de-intercalation are observed. In addition, the area of the CV curve increases when the applied potential is increased while retaining its original shape, indicating excellent reversibility and stability, important for practical devices. Fig. 9(b) conveys GCD curves for a symmetric device of copper pyrophosphate material at several current densities within the potential range of 0 to 1.6 V, which are decisive for analyzing rate capability and specific capacitance. The given diagram contemplates GCD data for five various current densities. The curve at lower current density (1 A g−1) exhibits much longer charge/discharge durations, indicating higher energy storage per cycle. The current density increases, and the discharge time in the symmetric device is noticeably shortened, which is expected due to accelerated ion transport. (a) Cyclic voltammogram, (b) galvanic charge–discharge profile, (c) specific capacitance at various current densities, (d) Ragone plot of α-Cu2P2O7 material. The following eqn (8) is used to calculate specific capacitance from GCD for a symmetric device:53,568 Fig. 9(c) provides the graph of current density in relation to capacitance. The values of specific capacitance (Csp) are 225, 203, 195, 182, and 172 F g−1 for current densities of 1, 1.1, 1.2, 1.3, and 1.4 A g−1, respectively. This analysis clearly shows that the electrode material α-Cu2P2O7 maintains notable capacitive behavior over a range of current densities, supporting its application for high-rate energy storage in a symmetric device. Fig. 9(d) illustrates the Ragone plot for the device, demonstrating the relationship between energy density and power density, with eqn (4) and (5) used to calculate both parameters. The energy density diminishes from 80 to 70 Wh kg−1, while the power density escalates from 3200 to 4480 W kg−1, when current density increases from 1 to 1.4 A g−1. This behavior highlights the device's have superior SCs performance. The cyclic stability of the α-Cu2P2O7 symmetric SCs was measured at a current density of 1.5 A g−1, as illustrated in Fig. 10(a). Eqn (6) and (7) were used to calculate capacity retention and coulombic efficiency, respectively. α-Cu2P2O7 symmetric device retains 90% of its initial capacity after 10 000 continuous charge–discharge cycles. The reason behind the reduction in capacity retention is the reduced charge and discharge time during cycling stability. Moreover, the coulombic efficiency after the cycling stability stood at 88%, exhibiting the high electrochemical stability of the synthesized α-Cu2P2O7 material. (a) Capacity retention and coulombic efficiency measurement for 10 000 charge discharge cycle (b) EIS of before and after stability with fitted circuit (c) b value of cathodic current (d) k value of cathodic current of α-Cu2P2O7 material. Fig. 10(b) depicts the EIS graph before and after cyclic stability. An associated fitted circuit is shown in the figure's inset. Table 4 compares the values of associated circuit elements before and after stability. The values of Rs, Rct, CPEDL and W were increased from 1st cycle to the 10 000th cycle. In symmetric SCs device, the Rct value is increased due to a decrease in available active sites at the interface between the electrode and electrolyte, which decreases the overall performance of the device. The EIS data, which are collected before and after cycling stability, corelates well with the decrease in stability of SCs device.4,56 Table 4Fitted values of circuit elements for the 1st and 10 000th cycles for symmetric SCsα-Cu2P2O7//α-Cu2P2O7 R s (Ω) R CT (Ω)CPEDL (S sn) W (Ω s−1/2)1st67.380.94567.78 × 10−58.65 × 10−310 000th104.471.200510.38 × 10−510.504 × 10−3 Fitted values of circuit elements for the 1st and 10 000th cycles for symmetric SCs The charge contribution and distribution from surface capacitive and diffusion-controlled processes were determined using Dunn's technique. In practical application, symmetric SCs may accumulate a total charge that is composed of three components, which include cation and anion insertion (intercalation pseudo capacitance), charge transfer with surface atoms (surface redox pseudo capacitance), and the double layer effect with all potential explanations for non-faradic processes. Fig. 10(c) shows the interaction between log(i) and log(v) during cathodic scanning. The above curve is fitted using the power law equation,9i = avbwhere i represents current, v represents scan rate while a and b are adjustable constants. The b value lies between 0.5 and 1, indicating that the charge storage mechanism of material involves a combination of diffusion-controlled faradaic processes and surface capacitive contributions, with moderate dominance of surface capacitive behavior. This mixed mechanism is characteristic of pseudocapacitive material electrodes contributes to both the high specific capacitance and good rate capability observed.53,56 The current's response at a fixed potential, i(V), is a balance between diffusion-controlled insertion (k2) and surface capacitive (k1) mechanisms, as illustrated in the equation below.10 The following equation was obtained by dividing both sides by the square root of the scan rate:11 The surface capacitance is denoted by k1ν, and the diffusion contribution current is denoted by k2ν1/2. Fig. 10(d) shows a linear graph comparing the square roots of current [i(V)/ν1/2] and scan rate [ν1/2] to determine k1 and k2 (slope and y-axis intercept, respectively). The non-faradaic capacitive current of cyclic voltammograms was used to determine the electrochemically active surface area (ECSA). The currents are quantified as half the difference between the cathodic currents at a constant voltage (0.8 V). Afterwards, CV is used to measure the current at different scan rates. To determine the slope, plot the current (I) against the scan rate (v) (Fig. 11(a)). The double-layer capacitance (Cdl) is associated with the slope of the chart line.12I = vCdl (a) Double layer capacitance value (b) capacitive (%) and diffusive (%) bar chart (c) capacitive and diffusion distribution at 10 mV s−1 (d) capacitive and diffusion distribution at 100 mV s−1 of α-Cu2P2O7 material. The obtained Cdl was 14.98 mF. The ECSA of a sample is determined from the double-layer capacitance using the following equation:53,5613where, CS represents the specific capacitance of a sample or the capacitance of an atomically flat planar surface of the material per unit area. The Cs value used for ECSA calculation is 2.20 × 10−2 mF cm−2. The measured ECSA of the electrode is 0.68 cm2. Fig. 11(b) illustrates the contribution proportion of capacitive and diffusion currents in an α-Cu2P2O7 electrode at changing scan rates. The capacitive contribution is seen to steadily grow from 55% to 80% when the scan rate is increased from 10 mV s−1 to 100 mV s−1, but the contribution of diffusion falls from 45% to 20%. The capacitive and diffusion current patterns that appear in the CV curve at scan rates of 10 and 100 mV s−1 are displayed in Fig. 11(c) and (d). According to the above findings the surface capacitive current increases as a result of accelerated ion transport with increasing scan rate. Fig. 12(a) depicts the CV of a symmetric device linked in series, resulting in a 3.2 V potential window; charging and discharging capabilities are shown in Fig. 12(b). In addition, Fig. 12(c) depicts two symmetric devices coupled in series. Furthermore, (d-f) displays the lighted LED for 1 minute and 27 seconds. (a) CV of symmetric device connected in series (b) GCD of symmetric device connected in series (c) picture of two device connected in series (d to f) Pictures of illuminated 3 V LED light of α-Cu2P2O7 material. Table 5 contains the values of Cs for various Phosphate based materials, which enable a comparative examination. The novel synthesis of α-Cu2P2O7 by co-precipitation technique exhibits a larger potential window when compared with previously reported data. The α-Cu2P2O7 exhibited increased capacitance at lower current density. Additionally, the α-Cu2P2O7 symmetric SCs device delivered high energy density, proving its potential for use in practical applications. Table 5Comparison table of phosphorus-based materialaDevice assemblyMethodPotential window (V)Specific capacitance F g−1Energy density Wh kg−1Power density W kg−1StabilityReferencesMn3(PO4)2/GF//ACHT1.4287.63601000 58 CoNiPO//ACHT1.614945.842.22500 59 Ni1·62Cu1·35(PO4)2//ACHT1.652.1218.5316405000 4 Cu2P2O7//ACCBD1.1234.839.4108610 000 60 Cu2P2O7//ACHT1.611539.835826000 55 Cu2P2O7//CNFs (AC)ES1.714357.6911042000 46 Cu2P2O7//Cu2P2O7 (S)SILAR0.9102.511.5427604500 44 CuCNT//CuCNT (S)SILAR0.922525.417565000 36 α-Cu2P2O7//α-Cu2P2O7 (S)Co-PPT1.6225@1 A g−180@1 A g−13200@1 A g−110000This workaGF:– Graphene, CBD:– Chemical bath deposition, SILAR:– Successive ionic layer adsorption and reaction, CNF:– Carbon nano fibres, HT:– Hydrothermal, ES:– Electrospinning, Co-PPT:– Coprecipitation, AC:– Asymmetric device, S:– Symmetric device. Comparison table of phosphorus-based materiala GF:– Graphene, CBD:– Chemical bath deposition, SILAR:– Successive ionic layer adsorption and reaction, CNF:– Carbon nano fibres, HT:– Hydrothermal, ES:– Electrospinning, Co-PPT:– Coprecipitation, AC:– Asymmetric device, S:– Symmetric device. Conclusion A template-based co-precipitation synthesis was employed to develop a high-performance SCs electrode. The development of pyrophosphate with copper ions also preserved structural stability and strong adhesion during the electrochemical process. The monoclinic structure with the space group C12/c1 was confirmed by XRD analysis. FE-SEM images indicated the formation of an interconnected particle with a rough surface area that aids in ion transport. FTIR spectroscopy confirmed the bending vibrations of α-Cu2P2O7, while Raman spectroscopy validated the bond formation of α-Cu2P2O7. Consequently, the α-Cu2P2O7 electrode possesses exceptional electrochemical properties, such as an outstanding specific capacitance of 667 F g−1 at a current density of 5 A g−1, an excellent rate capability of 90% after 5000 cycles, and an 80% coulombic efficiency in a three-electrode system. Additionally, the α-Cu2P2O7 symmetric SCs reveal a specific capacitance of 225 F g−1 at a current density of 1 A g−1. The device offers energy and power densities of 80 Wh/kg and 3200 W kg−1, respectively. It also exhibits exceptional cycling stability, maintaining 90% of its capacitance and achieving 88% of coulombic efficiency after 10 000 charge–discharge cycles at a current density of 1.5 A g−1. Ultimately, the fundamentals of the α-Cu2P2O7 electrode enable the development of alternative α-Cu2P2O7 electrodes for energy storage devices and SCs, thereby expanding its potential applications. Author contributions Jay Patel; methodology, investigation, data curation, formal analysis, writing – original draft, software. Karan Modi, Pruthvi Patel, and Dharti Patel; data curation, visualization. Vanaraj Solanki; reviewing. Bhavin Patel; reviewing. Mitesh H. Patel; conceptualization, funding acquisition, resources, supervision, writing – review and editing. Conflicts of interest The authors confirm that there is no conflict of interest. Supplementary Material