Protocol for depositing transparent conductive Ta-doped SnO2 film by hollow cathode gas flow sputtering technology Authors: Fangfang Huo, Manuel Hartig, Bertwin Bilgrim Otto Seibertz, Nivin Alktash, Ruslan Muydninov, Can Wang, Peng Gao, Bernd Szyszka Published: 2024 ABSTRACT SummaryTransparent conductive Ta-doped SnO2 (SnO2: Ta) thin film with low surface roughness, low resistivity, and high carrier concentration is one potential alternative of commercial transparent conductive oxides (TCOs). Here, we present a protocol for fabricating tin oxide films by hollow cathode gas flow sputtering technology. We describe steps for preparing and cleaning substrate, and film deposition process on the fresh uncorroded float glass substrate. We then detail procedures for measuring the optical and electrical properties of the film.For complete details on the use and execution of this protocol, please refer to Huo et al.1Subject areas: physics, chemistry, material sciences Before you begin The protocol below describes the specific steps to deposit undoped SnO2 and Ta doped SnO2 (SnO2: Ta) films on glass substrate by hollow cathode gas flow sputtering (GFS) technology under pulsed mode with different substrate temperature. This protocol could be used as a reference or guideline of other thin film materials deposited by hollow cathode gas flow sputtering technique. The hollow cathode gas flow sputtering system (GFS) operates as a remote plasma tool. The sputtering is performed in Ar and the reactive gas is introduced in the afterglow of the hollow cathode plasma, where the sputtered particles are transported by forced convection. There for, in contrast to reactive magnetron sputtering, no transition mode process stabilization is necessary for deposition of high quality transparent conductive oxides (TCOs) films.2 Glass tin and air side detecting Timing: 30 min 1.Identify tin and air side of fresh uncorroded float glass substrate.a.Put glass on a flat surface.b.Operate tin side detector following manual.c.Make a mark ‘×’ on the tin side with diamond marker. Identify tin and air side of fresh uncorroded float glass substrate.a.Put glass on a flat surface.b.Operate tin side detector following manual.c.Make a mark ‘×’ on the tin side with diamond marker. a.Put glass on a flat surface. Put glass on a flat surface. b.Operate tin side detector following manual. Operate tin side detector following manual. c.Make a mark ‘×’ on the tin side with diamond marker. Make a mark ‘×’ on the tin side with diamond marker. Note: Protect glass surface and avoid scratch left on both surfaces. Glass cut Timing: 1 h 2.Cut glass substrate to desired dimension.a.Put glass tin side on bottom.b.Cut 10 cm × 10 cm × 3 mm glass to 3 cm × 3 cm × 3 mm.c.Make a mark ‘×’ on tin side of each 3 cm × 3 cm × 3 mm glass with diamond marker.d.Separate glass to small pieces glass following the scratch line with glass cut pliers. Cut glass substrate to desired dimension.a.Put glass tin side on bottom.b.Cut 10 cm × 10 cm × 3 mm glass to 3 cm × 3 cm × 3 mm.c.Make a mark ‘×’ on tin side of each 3 cm × 3 cm × 3 mm glass with diamond marker.d.Separate glass to small pieces glass following the scratch line with glass cut pliers. a.Put glass tin side on bottom. Put glass tin side on bottom. b.Cut 10 cm × 10 cm × 3 mm glass to 3 cm × 3 cm × 3 mm. Cut 10 cm × 10 cm × 3 mm glass to 3 cm × 3 cm × 3 mm. c.Make a mark ‘×’ on tin side of each 3 cm × 3 cm × 3 mm glass with diamond marker. Make a mark ‘×’ on tin side of each 3 cm × 3 cm × 3 mm glass with diamond marker. d.Separate glass to small pieces glass following the scratch line with glass cut pliers. Separate glass to small pieces glass following the scratch line with glass cut pliers. CRITICAL: It is necessary to put tissues on the bottom of glass to protect the surface during scratching. Put glass surface with scratched line on the center of round part with bulge when using glass cut pliers, the position of glass is shown in Figure 1. Glass cutting (A) Schematic of glass cutting with glass cut pliers. (B) Sample cutting. Substrate cleaning Timing: 90 min 3.Glass substrate cleaning.a.Clean glass with ethanol by ultrasonic cleaner, 15 min, room temperature.b.Clean glass with isopropanol by ultrasonic cleaner, 15 min, room temperature.c.Clean glass with deionized water by ultrasonic cleaner, 15 min, room temperature.d.Drying glass surface by N2 gun. Glass substrate cleaning.a.Clean glass with ethanol by ultrasonic cleaner, 15 min, room temperature.b.Clean glass with isopropanol by ultrasonic cleaner, 15 min, room temperature.c.Clean glass with deionized water by ultrasonic cleaner, 15 min, room temperature.d.Drying glass surface by N2 gun. a.Clean glass with ethanol by ultrasonic cleaner, 15 min, room temperature. Clean glass with ethanol by ultrasonic cleaner, 15 min, room temperature. b.Clean glass with isopropanol by ultrasonic cleaner, 15 min, room temperature. Clean glass with isopropanol by ultrasonic cleaner, 15 min, room temperature. c.Clean glass with deionized water by ultrasonic cleaner, 15 min, room temperature. Clean glass with deionized water by ultrasonic cleaner, 15 min, room temperature. d.Drying glass surface by N2 gun. Drying glass surface by N2 gun. Note: Use sample holder during cleaning process to protect glass surface. 4.Store glass substrate in sample box under air. Store glass substrate in sample box under air. CRITICAL: Sample box should be cleaned before store substrate. Avoid touching substrate surface during the whole cleaning process. Key resources table REAGENT or RESOURCESOURCEIDENTIFIERChemicals, peptides, and recombinant proteinsEthanolMicroChemicalsCAS Nr.: 64-77-5IsopropanolMicroChemicals(VLSI)CAS Nr.: 67-63-0Deionized waterClean room laboratory0.055 μS/cmSoftware and algorithmsEVABrukerV5.1OtherGlassSaint-Gobain GlassPLANICLEAR 30 cm × 30 cmUltrasonic cleanerBANDELIN SONOREXRK 102 HTin side detectorTS1420Line-poweredGlass cut pliersSilberschnittBO 700.0ASn targetAvaluxe International GmbHID 40 mm, OD 50 mm, L 70 mmTa targetAvaluxe International GmbHID 40 mm, OD 50 mm, L 5 mmHollow cathode gas flow sputtering systemFraunhofer Institute for Surface Engineering and Thin FilmsKL-GFS-RQ50.LCG.TA40Four-point probeVeeco Instruments Inc.FPP-5000Hall measurementLake Shore CryotronicsM91UV/VIS/NIR spectrometerPerkinElmerLambda 1050+Atomic force microscopy (AFM)Spectral InstrumentsNTEGRA IIScanning electron microscope (SEM)ZeissDSM 982 GEMINIWavelength dispersive X-ray spectroscopy (WDXS)HitachiS-2700X-ray diffractionBrukerD8 Discover Materials and equipment The glass substrate cleaning process with ultrasonic cleaner should be operated in fume hood in chemical lab. The Sn and Ta targets should be stored under vacuum. The experiment program is shown in Figure 2. Note: Check quantity and quality of materials before experiment to get better perception in considering the same steps of experiments. CRITICAL: Ethanol and Isopropanol are hazardous chemical due to their inflammability. One should wear protective glass, gloves and clothing to operate glass cutter due to the splash of glass. Alternatives: The cleaning process with other chemicals, for example acetone and other special glass cleaning solutions, can be used to clean substrate surfaces.3 The glass cutter can be replaced by other cutting methods, for example laser cutter.4 The general chemicals used for substrate cleaning process in this protocol can be replaced by those from other sources. The instruments applied for film property characterization applied in this protocol can be replaced by those which have similar functions.3,5,6,7 For example, another ultraviolet visible near infrared (UV/VIS/NIR) spectrometer, four-point probe and hall measurement setup. The experiment program can be changed by other experiment program with other sputtering system which has similar functions. For example, replace O2 flow rate series by Ar flow rate series to study the influence of plasma conditions on film properties, replace in situ substrate temperature series by post annealing series. Experiment program Step-by-step method details Test deposition Timing: 2.5 h Test deposition should be done before the first sample deposition, to make sure the device runs under normal conditions. The following steps describe the process of preparation work before experiment starts, it works as a tiny device debugging. Figure 3 shows the overview of hollow cathode gas flow sputtering (GFS) system windows control center (WinCC), and Figure 4 shows schematic of film deposition process. Note: Wear glove during sample preparation and inside chamber operation process. Avoid touching film surface. CRITICAL: The following steps can be only operated when the gases (Ar, N2 and O2), cooling water and electricity supply normally in the sputtering lab, and there is no machine defect. After the whole procedure finished, test sample to check if sheet resistance stays in the expected range. If it is in the expected range, then continue the following protocol steps, if not, contact engineer to find out issues. 1.Turn on gas valve.a.Turn on the main gas valve.b.Turn on Ar, N2 and O2 valve. Turn on gas valve.a.Turn on the main gas valve.b.Turn on Ar, N2 and O2 valve. a.Turn on the main gas valve. Turn on the main gas valve. b.Turn on Ar, N2 and O2 valve. Turn on Ar, N2 and O2 valve. 2.Turn on cooling machine. Turn on cooling machine. 3.Click button 1 and button 2, vent chamber and vacuum line by filling with N2. Click button 1 and button 2, vent chamber and vacuum line by filling with N2. 4.Open chamber door, the structure of hollow cathode gas flow sputtering (GFS) system vacuum chamber is shown in Figure 5A. Open chamber door, the structure of hollow cathode gas flow sputtering (GFS) system vacuum chamber is shown in Figure 5A. 5.Insert target. Insert target. Note: The total length of target is 60 mm ± 0.1 mm. If the target is a combination of several pieces, make sure each piece contact with other well, there is no clear space between every target piece. The shape of the target is shown in Figures 5B and 5C. 6.Insert substrate. Insert substrate. Note: For room temperature and heated substrate temperature under 150°C, substrate could be fixed by heat resistant tape. For heated substrate temperature over 150°C, substrate should be fixed with matched substrate holder. CRITICAL: Wear fresh gloves to move and insert substrate, avoid touching the sample surface which the film will be deposited on. After sample is fixed, use N2 gun clean sample surface to avoid substrate contamination on surface. 7.Adjust the distance between target and substrate. Adjust the distance between target and substrate. 8.Move substrate holder to position 5. Move substrate holder to position 5. 9.Close chamber door. Close chamber door. 10.Click button 3 and button 4, vacuum the chamber until 2 × 10 –2 mbar. Click button 3 and button 4, vacuum the chamber until 2 × 10 –2 mbar. 11.Turn on heater power, click button 5 and button 6 to start heating process. Turn on heater power, click button 5 and button 6 to start heating process. Note: Heating process is designed in advance before every experiment. 12.Click button 5 and button 6 again to end heating process. Click button 5 and button 6 again to end heating process. 13.Click button 9 and button 10, fill in Ar and reactive gas O2 to chamber. Click button 9 and button 10, fill in Ar and reactive gas O2 to chamber. Note: After filling in Ar and O2, wait the vacuum value stays stable. 14.Click buttons 9, 10 and 11 in sequence, to generate plasma and start pre – sputtering process. Click buttons 9, 10 and 11 in sequence, to generate plasma and start pre – sputtering process. 15.Move substrate holder to position 3. Move substrate holder to position 3. 16.Start depositing process with designed parameters. Start depositing process with designed parameters. 17.To end the deposition process, click on button 11, 10, and 9 in sequence. To end the deposition process, click on button 11, 10, and 9 in sequence. 18.Click button 8 and button 7 to turn off the Ar and O2 gas flow. Click button 8 and button 7 to turn off the Ar and O2 gas flow. 19.Click button 4 and button 3 to stop vacuum chamber. Click button 4 and button 3 to stop vacuum chamber. 20.Wait substrate temperature cooling down to be below 70°C, click button 1 and button 2, open chamber door, and take sample out. Wait substrate temperature cooling down to be below 70°C, click button 1 and button 2, open chamber door, and take sample out. Note: Please follow the sputtering lab security rules carefully. When it is necessary, wear the mask when opening the chamber to take sample out to avoid detrimental hazardous situation. 21.Close chamber door. Close chamber door. 22.Click button 3 and button 4 to vacuum system again. Click button 3 and button 4 to vacuum system again. 23.After chamber vacuum pressure reach 10 –2 mbar range, click button 3 and button 4 turn vacuum system off. After chamber vacuum pressure reach 10 –2 mbar range, click button 3 and button 4 turn vacuum system off. 24.Turn heater power off, turn cooling system off, close all gas valves. Turn heater power off, turn cooling system off, close all gas valves. 25.Measure sheet resistance of test sample. Measure sheet resistance of test sample. Hollow cathode gas flow sputtering (GFS) system Hollow cathode gas flow sputtering (GFS) system windows control center (WinCC) overview. Button 1: vent chamber. Button 2: vent vacuum line. Button 3: open/close main vacuum valve. Button 4: start vacuum pumping. Button 5: Substrate holder temperature control. Button 6: Pretreatment temperature control. Button 7: Ar flow rate control. Button 8: O2 flow rate control. Button 9: Generator 1 main switch. Button 10: Generator 2 main switch. Button 11: GFS Plasma control. Schematic illustration of hollow cathode gas flow sputtering deposition process Hollow cathode gas flow sputtering system and target Figure reprinted with permission from Huo et al., 2024.1 (A) The structure of hollow cathode gas flow sputtering system vacuum chamber: source (1), pre-heating (2), and substrate holder (3). Position 5 is used for preheating, position 3 is used for film deposition. S1 is pretreatment position (VBS)_intern sensor, S2 is pretreatment position (VBS)_extern sensor, S3 is substrate holder (SH)_ intern sensor, S4 is substrate holder (SH)_extern sensor. (B) Top view of target. (C) Side view of target. Deposition SnO2 film Timing: 30–120 min (per sample, varies by deposition parameter) The follow steps describe the deposition process of SnO2 film on the fresh uncorroded float glass substrate based on the procedure of “Test deposition”. Five series with different substrate temperature are designed for SnO2 film deposition: I: room temperature; II: 50°C; III: 110°C; IV: 270°C; and V: 400°C. Note: Wear glove during sample preparation and inside chamber operation process. Avoid touching film surface. 26.Design heating process, as is shown in Figures 6A–6D. Design heating process, as is shown in Figures 6A–6D. Note: Room temperature deposition does not need heating process. In this protocol, substrate temperature is defined by the temperature detected by substrate holder (SH)_extern sensor, which is marked with red dot in the Figure 6. The corresponding input value to heating system is marked with black dot, which are detected by pretreatment position sensor (VBS)_intern sensor and substrate holder (SH)_intern sensor. CRITICAL: From 200°C heater should be heated step by step every 100°C to protect whole heating system not to overwork. 27.Insert Sn target. Insert Sn target. 28.Insert glass substrate, adjust the distance between target and substrate to 4 cm. Insert glass substrate, adjust the distance between target and substrate to 4 cm. Note: Make sure glass substrate is fixed stable and at the center of substrate holder. 29.Pump chamber pressure to 2 × 10 –2 mbar. Pump chamber pressure to 2 × 10 –2 mbar. 30.Move sample to position 5 and start heating process which is shown in Figure 6. Move sample to position 5 and start heating process which is shown in Figure 6. Note: Skip step 31 when do room temperature deposition, directly following the deposition parameters described in step 32 to prepare films. 31.After heating process completed, move sample to position 3. After heating process completed, move sample to position 3. 32.Start deposition process.a.Ar flow rate is 1000 sccm.b.O2 flow rate is 5–45 sccm.Note: The step of O2 flow rate is 5 sccm.c.Operating pressure during sputtering is held at 3.2 × 10 –1 mbar.d.Operating power is 250 W.e.Pre- sputtering time is 5 min.Note: Pre – sputtering step here is to clean target surface.f.Pulse mode reverse voltage is 100 V, frequency is 100 kHz, time is 2 μs.g.Deposition time is 60 s to deposit ∼350 nm SnO2 film, as deposition rate is 6 nm/s. Start deposition process.a.Ar flow rate is 1000 sccm.b.O2 flow rate is 5–45 sccm.Note: The step of O2 flow rate is 5 sccm.c.Operating pressure during sputtering is held at 3.2 × 10 –1 mbar.d.Operating power is 250 W.e.Pre- sputtering time is 5 min.Note: Pre – sputtering step here is to clean target surface.f.Pulse mode reverse voltage is 100 V, frequency is 100 kHz, time is 2 μs.g.Deposition time is 60 s to deposit ∼350 nm SnO2 film, as deposition rate is 6 nm/s. a.Ar flow rate is 1000 sccm. Ar flow rate is 1000 sccm. b.O2 flow rate is 5–45 sccm.Note: The step of O2 flow rate is 5 sccm. O2 flow rate is 5–45 sccm.Note: The step of O2 flow rate is 5 sccm. Note: The step of O2 flow rate is 5 sccm. c.Operating pressure during sputtering is held at 3.2 × 10 –1 mbar. Operating pressure during sputtering is held at 3.2 × 10 –1 mbar. d.Operating power is 250 W. Operating power is 250 W. e.Pre- sputtering time is 5 min.Note: Pre – sputtering step here is to clean target surface. Pre- sputtering time is 5 min.Note: Pre – sputtering step here is to clean target surface. Note: Pre – sputtering step here is to clean target surface. f.Pulse mode reverse voltage is 100 V, frequency is 100 kHz, time is 2 μs. Pulse mode reverse voltage is 100 V, frequency is 100 kHz, time is 2 μs. g.Deposition time is 60 s to deposit ∼350 nm SnO2 film, as deposition rate is 6 nm/s. Deposition time is 60 s to deposit ∼350 nm SnO2 film, as deposition rate is 6 nm/s. 33.Repeat step 17 to step 20, until take sample out. Repeat step 17 to step 20, until take sample out. Note: When it is necessary, wear the mask when opening the chamber to take sample out to avoid detrimental hazardous situation. 34.Insert next substrate, repeat step 30 to step 34 to prepare the second sample. Insert next substrate, repeat step 30 to step 34 to prepare the second sample. 35.Repeat step 35 for multiple times and complete the depositions for all samples which are designed for temperature series and O2 flow rate series. Repeat step 35 for multiple times and complete the depositions for all samples which are designed for temperature series and O2 flow rate series. 36.Repeat step 21 to step 24 to finish deposition. Repeat step 21 to step 24 to finish deposition. Heating process of different substrate temperature Heated substrate holder temperature detected by substrate (SH)_extern sensor is marked with red dot in the figure. (A) 50°C. (B) 110°C. (C) 270°C. (D) 400°C. Deposition SnO2: Ta film Timing: 30–120 min (per sample, varies by deposition parameter) The follow steps describe the deposition process of SnO2: Ta film on the fresh uncorroded float glass substrate based on the procedure of “Deposition SnO2 film”. Five series with different substrate temperature are also designed for SnO2: Ta film deposition: I: room temperature; II: 50°C; III: 110°C; IV: 270°C; and V: 400°C. Note: Wear glove during sample preparation and inside chamber operation process. Avoid touching film surface. CRITICAL: To compare SnO2: Ta films with SnO2 film, expect the target is different, other parameters should keep same with SnO2 film. Substrate heating process is same as the heating process of SnO2 film which is shown in Figure 6. 37.Insert Ta target, the 5 mm doping ring. Insert Ta target, the 5 mm doping ring. Note: Make sure Ta ring is at the beginning of plasma direction, the 3-dimension (3D) Ta ring and plasma direction is shown in Figure 7. 38.Insert Sn ring. Insert Sn ring. 39.Repeat steps from 28 to 36 to complete the deposition of SnO2: Ta films. Repeat steps from 28 to 36 to complete the deposition of SnO2: Ta films. 3D Ta doping ring and Sn target used for SnO2: Ta films deposition Measuring optical and electrical property of the films Timing: depends on measurement method The following steps describe the process of measurements of optical and electrical properties. Note: For all measurement wear gloves to move sample and avoid touching sample surface. 40.Apply a UV/VIS/NIR spectrometer to measure total transmittance and reflectance of prepared films.a.To measure the total transmittance, put sample at the front window of the integrating sphere, and put white standard at the back window of integrating sphere.b.To measure the reflectance, put sample at the back window of integrating sphere. Apply a UV/VIS/NIR spectrometer to measure total transmittance and reflectance of prepared films.a.To measure the total transmittance, put sample at the front window of the integrating sphere, and put white standard at the back window of integrating sphere.b.To measure the reflectance, put sample at the back window of integrating sphere. a.To measure the total transmittance, put sample at the front window of the integrating sphere, and put white standard at the back window of integrating sphere. To measure the total transmittance, put sample at the front window of the integrating sphere, and put white standard at the back window of integrating sphere. b.To measure the reflectance, put sample at the back window of integrating sphere. To measure the reflectance, put sample at the back window of integrating sphere. CRITICAL: Calibration should be done before transmittance and reflectance measurement. 41.Choose Bragg Brentano geometry to do XRD measurement. Choose Bragg Brentano geometry to do XRD measurement. 42.Put sample on test plate, measure edge and center film position sheet resistance by using four-point probe, calculate the average value as the film sheet resistance Rsh (Ω/ □), mark the films which are conductive. Put sample on test plate, measure edge and center film position sheet resistance by using four-point probe, calculate the average value as the film sheet resistance Rsh (Ω/ □), mark the films which are conductive. 43.Follow step 2, cut conductive samples to 1.5 cm × 1.5 cm to hall measurement. The needles contacts four corners edge of sample. When contact well, change the direction of magnet to get film resistivity, mobility and carrier concentration. Follow step 2, cut conductive samples to 1.5 cm × 1.5 cm to hall measurement. The needles contacts four corners edge of sample. When contact well, change the direction of magnet to get film resistivity, mobility and carrier concentration. 44.Go for scanning electron microscope (SEM) to study the morphology and cross section of the films. Go for scanning electron microscope (SEM) to study the morphology and cross section of the films. Note: To ensure sample could be reused and remeasured after SEM measurement, do SEM without any coating on sample surface. Expected outcomes The operating pressure of sputtering system is at 3.2 × 10 –1 mbar with inputting different O2 flow rate from 5 sccm to 45 sccm. For all experiments, the time needed to pump chamber pressure to background 2 × 10 –2 mbar is similar. The sample under room temperature is not conductive, with the increasing of substrate temperature, film turns to be conductive. The conductivity of the film is changing with different O2 flow rates. If the film looks dark at the lowest O2 flow rate at 5 sccm, it should turn to be transparent by eyes after increasing the O2 flow rate to next level. Since the deposition time is controlled at 60 s, the thickness of all films is between 300 and 400 nm. The doping effect could be seen at least in one temperature series, by observing the conductivity of Ta doped SnO2 film is higher than that of SnO2 film. With crystallized film, which is detected by X-ray diffraction (XRD) measurement, the growing structure shows like collum grown crystal, which is shown in Figure 8A. Transmittance of SnO2 and SnO2: Ta is shown in Figure 8B. The peak positions in XRD pattern of crystallized films are matched with references, which are shown in Figure 8C. The host material structure of SnO2 is not changed by Ta doping since the atom ratio of Ta in SnO2: Ta film is small, 2.11% in SnO2: Ta film with 270°C substrate temperature, corresponding 1.608% of C, 69.316% of O, 0.47 of Ar, 26.496% of Sn. And Ta doping influences the film crystallinity and grown structure. Diffractive (110), (200) and (211) peaks move to a smaller 2θ value could be observed under different oxygen flow rate, due to the radius of Ta5+ is smaller than that of Sn4+, which is shown in Figures 8D–8F. The diffraction peaks of the thin films differ under different oxygen flow rates comes from the correlated different plasma conditions with high plasma density in GFS technology and reactive gas oxygen during deposition process, which could influence the film grown structure. Roughness of the deposited film at 25 sccm oxygen flow with different substrate temperature is listed in Table 1. Note: For oxides other than SnO2, oxygen flow rate and other deposition parameters could be established based on the literature overview work from other researchers and groups, and different trial experiments following the experiment steps which are describe in this protocol. The deposited successful tin oxide film (A) Collum structure of tin oxide film, scale bar is 300 nm. (B) Transmission of SnO2 and Ta doped SnO2 film. Insert is the photo of prepared film. (C) XRD pattern of crystallized tin oxide films. (D) (110) peak shift. (E) (200) peak shift. (F) (211) peak shift. Table 1AFM measurements on a 1 μm × 1 μm large area for samples deposited at 25 sccm oxygen flowSampleRoughness (RMS)SnO2 @ 270°C6.02 nmSnO2 @ 400°C4.08 nmSnO2: Ta @ 270°C3.01 nmSnO2: Ta @ 400°C2.32 nm AFM measurements on a 1 μm × 1 μm large area for samples deposited at 25 sccm oxygen flow Limitations This protocol should be applied carefully since there are limitations. The deposition parameters for tin oxide films, for example, target power, O2 flow rate, substrate temperature, and deposition time, etc. for the equipment in this protocol may be not applicable for other sputtering equipment with similar functions. Due to the limitation of the equipment, only one sample in this protocol could be deposited one time. With high temperature substrate deposition, heating and cooling process takes time. There is also the limitation of the kind of glass substrate used in this protocol. The tin oxide film structure and property may not be applicable for other substrates.8 Troubleshooting Problem 1 Plasma cannot be generated successfully. After filling in Ar, switch on generator, plasma cannot be seen through the chamber window, there is no power, voltage and current value in WinCC window (steps 15, 33 and 39). Potential solution Use handheld vacuum cleaner to clean anode surface and check the insertion of target. For one piece 60 mm target, make sure the target surface and anode surface are in one plane. There is no gap between the cover and anode and cathode (target), which is shown in Figure 9. Target installation (A) Wrong installation. (B) Correct installation. For several integrated targets, make sure each pieces contact well with others. For the thin target ring (< 5 mm), insert slowly and carefully to forbid the rotating in anode. Problem 2 Heating curves shows not correctly or stay at 0 during heating process in WinCC window (steps 11 and 30). Potential solution Check the contact of sensor cable at substrate holder and chamber wall. Substrate holder (SH)_extern sensor cable at substrate holder back side maybe is damaged due to the movement of substrate holder or the incorrectly operation of the position changing of substrate holder to fix and take sample out. Problem 3 Target edge color is different with the color in target middle position by visual. (e.g., step 5). Potential solution Sand target internal surface with sandpaper, remove the particles on target surface. Target surface status could be changed due to long time deposition. Besides pre-sputtering, remove target surface by physical and mechanical way is also possible to make sure the target is under metallic status. Problem 4 Film is not deposited on the center of the substrate. (step 28). Potential solution Make sure sample is stuck in the substrate holder at the matched position. Resource availability Lead contact Further information and requests for resources should be directly to and will be fulfilled by the lead contact, Bernd Szyszka (bernd.szyszka@tu-berlin.de). Technical contact Questions about the technical specifics of performing the protocol should be directed to and will be fulfilled by the technical contact, Fangfang Huo (fangfang.huo@tu-berlin.de) and Bernd Szyszka (bernd.szyszka@tu-berlin.de). Materials availability This study did not generate new unique reagents. Data and code availability This study did not generate/analyze datasets/code. Acknowledgments This work received financial support from Technical University Berlin, and from X-ray diffractometer used by the Deutsche Forschungsgemeinschaft (DFG, German Research Foundation)—grant number AOBJ 649257. We thank the support from Kompetenzzentrum Photovoltaik (PVcomB), Helmholtz-Zentrum Berlin für Materialien und Energie GmbH (HZB). Author contributions F.H. conducted the experiments, analyzed data, and wrote the manuscript. B.S. supervised the whole work and provided experiment resources. M.H. cut glasses and samples and provided sputtering lab support. B.B.O.S. provided XRD lab support and AFM studies. N.A. and R.M. provided sputtering lab support. C.W., P.G., and B.S. contributed to manuscript editing. Declaration of interests The authors declare no competing interests. Contributor Information Fangfang Huo, Email: fangfang.huo@tu-berlin.de. Bernd Szyszka, Email: bernd.szyszka@tu-berlin.de. References Associated Data Data Availability Statement This study did not generate/analyze datasets/code.