Antibacterial activity of copper-decorated CeO2 nanoparticles and preparation of antifouling polyethersulfone surface Authors: Lokman Şener, Sadin Özdemir, M. Serkan Yalçın, Mehmet Gülcan, Nadir Dizge Published: 2024 ABSTRACT Cerium oxide NPs (nano-CeO2), with notable performance in various biological tests like redox activity, free radical scavenging, and biofilm inhibition, emerge as significant candidates to address issues in related areas. In this research, copper-decorated nano-CeO2 (Cu@nano-CeO2) were first synthesized and then characterized using advanced techniques such as SEM-EDX, XRD, XPS, BET, and ICP-OES. The biochemical properties of the obtained Cu@nano-CeO2 nanostructure and its performance in polyethersulfone (PES) membranes were thoroughly investigated in this research study. The free radical scavenging effect of Cu@nano-CeO2 at 100 mg/L concentration was determined as 100 % with the same activity as the reference compounds Trolox and ascorbic acid. It enhanced 2.9-fold α-amylase enzyme activity at 50 mg/L. Plasmid DNA was completely degraded at 100 mg/L concentration. Cu@nano-CeO2 provided significant inhibition against tested bacterial and fungal strains, especially Gram-positives than Gram-negatives and fungus. Anti-biofilm activity was determined against S. aureus and P. aeruginosa as 98.3 and 82.1 %, respectively. Furthermore, E. coli inhibition activity of PES/Cu@nano-CeO2 1.0 wt% membrane was determined as 100 %. Owing to the promising results obtained, we can suggest that Cu@nano-CeO2 can be used in wastewater treatment. Introduction Cerium (Ce) is one of the best elements representing rare earth elements due to its unique chemical/physical properties and distinctive outer electron configuration ([Xe]4f15d16s2). Its abundant presence in the Earth's crust (66.5 ppm) has made the utilization of Ce-based compounds notably prominent in recent years due to their price advantage. Ce compounds find applications in various industrial sectors including magnets, alloys, and catalysis. Among these Ce compounds, cerium oxide (CeO2) has garnered the most interest as a star material in academic research or practical fields [1,2]. CeO2 nanoparticles (NPs) have particularly attracted intense interest in nanotechnology due to their beneficial applications as catalysts, fuel cells, and antioxidants in biological systems [[3], [4], [5], [6]]. Generally, cerium is known to exist in two oxidation states: Ce3+ and Ce4+. Therefore, cerium dioxide can exist in two different oxide forms in bulk material: CeO2 (Ce4+) or Ce2O3 (Ce3+) [7,8]. At the nano scale, cerium oxide possesses a cubic fluorite structure, and both Ce3+ and Ce4+ can coexist on its surface. The presence of Ce3+ leads to a charge deficiency compensated by oxygen vacancies within the cage, thus CeO2-NPs inherently contain oxygen defects [9]. These oxygen defects are actually designated as active sites for catalytic activities. As the particle size decreases, the concentration of oxygen defects increases, thereby CeO2-NPs exhibit enhanced redox properties compared to bulk materials [10]. Additionally, it's noted in the literature that the presence of mixed valence states plays a significant role in the removal of reactive oxygen and nitrogen species. Furthermore, it has been found that CeO2-NPs are effective against pathologies associated with chronic oxidative stress and inflammation. However, recently, it has been reported that CeO2-NPs exhibit fascinating properties as a material with multiple enzyme-like activities, including superoxide dismutase, catalase, and oxidase, in very important biological areas such as bioanalysis, biomedicine, and drug delivery [8,[11], [12], [13], [14], [15], [16]]. It is known that all these applications are derived from the rapid transition between the oxidation states of Ce3+ and Ce4+ [7]. The surface Ce3+:Ce4+ ratio is influenced by the microenvironment. Therefore, the adopted microenvironment and synthesis method also play an important role in determining the biological activity and toxicity of CeO2-NPs. Literature studies indicate that solution precipitation, sonochemical, hydrothermal, solvothermal, ball milling, thermal decomposition, spray pyrolysis, thermal hydrolysis, and sol-gel methods are used to synthesize CeO2-NPs [8,[14], [15], [16]]. Nanomaterials, defined as structures ranging from 1 nm to 100 nm, are being investigated in various scientific fields such as physics, chemistry, biology, medicine, pharmacy, and materials science due to their different optical and electronic properties from their bulk counterparts [[17], [18], [19]]. Reducing the particle size unveils the superior characteristics of these materials, enabling the development of new and advanced applications in fields such as communication, energy storage, sensing, data storage, optics, transmission, environmental protection, cosmetics, biology, and medicine. In recent years, significant efforts have been made to produce many nanomaterials with controlled morphologies, shapes, and sizes [15]. Metal NPs, which have a higher surface-to-volume ratio compared to their bulk counterparts, contain more catalytically active atoms on their surfaces. Thus, the wide surface areas and high surface energies make metal NPs thermodynamically unstable against aggregation in bulk form. In this context, suitable protective ligands or polymers are widely used in their synthesis to prevent their aggregation. However, even in the presence of the best stabilizing agents, the eventual agglomeration of metal NPs into bulk remains the most critical issue that needs to be overcome in applications. Additionally, obtaining pure active metal surfaces by avoiding surface contamination from surface-protecting groups, which often leads to reduced effectiveness due to the blocking of active sites, is another critical issue. In this regard, using porous and nano-sized support materials as host materials for the immobilization of guest metal NPs allows the production of active sites without specific surface-active substances, along with the advantages of preventing particle aggregation [[20], [21], [22]]. The general definition of membrane fouling is the accumulation and deposition of unwanted elements inside or on the surface of membranes. Particles in solution, partially soluble organic and/or inorganic macromolecules, and/or biological microorganisms could all be among the materials that have been deposited. Membrane fouling, thus, is an inevitable phenomenon in membrane-based water treatment processes and can seriously harm the processes' functionality, sustainability, and viability from an economic standpoint. The numerous physical and chemical interactions that occur between the membrane surface and different feed contents result in fouling mechanisms [[23], [24], [25]]. Foulant deposition and fouling layer formation are significantly influenced by the properties of the membrane surface, such as charge, chemistry, hydrophobicity/hydrophilicity, and shape [26]. Therefore, modifying these attributes through a suitable membrane surface modification technique offers the most effective means of enhancing the antifouling performance of membranes. Common surface modification techniques encompass reducing the roughness of the membrane surface, enhancing its hydrophilicity, and introducing antiadhesive monomers, polymers, or nanoparticles onto the membrane surface [[27], [28], [29], [30], [31]]. The development of antifouling coatings for membranes has benefited substantially from current developments in nanotechnology, polymer science, and biomimetic surface design. In order to enhance the antifouling capabilities of membranes, metal and metal oxide nanoparticles (NPs) such as Ag, Fe3O4, TiO2, and WS2 have been employed in membrane manufacture and/or modification during the last decade. Additionally, carbon-based nanomaterials such as CNTs, graphene, GO, and polymeric NPs have attracted intensive research interests in the antifouling capabilities of membranes [32]. Motivated by the superior properties of cerium oxide and metal nanoparticles outlined above, in this research study, copper-decorated nano-CeO2 (Cu@nano-CeO2) was first prepared and characterized using a combination of various techniques. Subsequently, the biochemical properties and the performance of polyethersulfone (PES) membrane of Cu@nano-CeO2 nanostructure were investigated. Materials and method Materials Copper (II) chloride dihydrate (CuCl2∙2H2O), cerium (IV) oxide (CeO2; nanopowder, <25 nm particle size), and N-methyl-2-pyrrolidine (NMP) were acquired from Sigma-Aldrich for experimental investigations and were utilized without prior treatment. Polyethersulfone (PES) used as a polymer (Ultrasound E 6020 P) was kindly provided form BASF Company in Turkey. Likewise, all solvents employed in the experimental studies were of high purity, obviating the need for preliminary purification. Synthesis of Cu@nano-CeO2 The decoration of Cu NPs on the nano-CeO2 surface was carried out through wet impregnation-reduction steps [33,34]. For this purpose, a solution of CuCl2∙2H2O salt containing 2 % Cu metal was mixed with nano-CeO2 at 298 K and 750 rpm for approximately 4 h. Then, an aqueous solution of NaBH4 was added to the mixture to reduce the Cu metals on the nano-CeO2 surface. After the reduction process was completed, the mixture was centrifuged to isolate the solid part. The solid product was washed several times with water to remove potential impurities and then dried overnight in a vacuum oven set at 80 °C. Synthesis of Cu@nano-CeO2 blended PES membrane PES membranes both pristine and functionalized were synthesized using the phase inversion approach. Initially, PES beads were dried at 70 °C in an oven for 2 h. After that, Cu@nano-CeO2 were dissolved uniformly in the NMP solvent for 10 min in an ultrasonic water bath and PES beads were added to the final mixture. Overnight at 60 °C in an incubator, PES beads were allowed to dissolve completely in the solution while being shaken. Additionally, PES beads (14 %, w/w) were dissolved in NMP solvent at 60 °C to prepare the casting solution for the pristine membrane. In order to synthesis blended composite membranes, Cu@nano-CeO2 was added to the casting solution at varying weight percentages (0.5, 1.0, and 2.0 wt%) Then, air bubbles were eliminated from the polymer solution by sonicating it for duration of 20 min. A 200 μm thick casting blade was used to disseminate the bubble-free membrane solutions at a speed of 100 mm/s across the glass layer. To precipitate the polymer, the glass plate was immerged in a coagulation bath containing deionized water. After the polymer was precipitated by immersing the glass plate in a coagulation bath with deionized water, the membranes were phase-transformed and the residual solvent was removed by immersing the plate in distilled water for at least an overnight. Characterization The characterization of the Cu@nano-CeO2 nanostructure involved several techniques. A Zeiss Sigma 300 scanning electron microscope was utilized for scanning electron microscopy (SEM) and scanning electron microscopy-energy dispersive X-ray spectroscopy (SEM-EDX) analyses. PANalytical Empyrean X-ray diffractometer with Cu-Kα radiation (wavelength 1.54 Å, 40 kV, 55 mA) was employed for obtaining P-XRD patterns. Surface chemistry details of the Cu@nano-CeO2 nanostructure were acquired using a Kratos AXIS Ultra spectrometer for XPS analysis with monochromatic Al-Kα radiation (1486.6 eV, the X-ray tube operating at 15 kV and 350 W, and pass energy of 23.5 eV). The C 1s photoelectron line (binding energy = 284.6 eV) was employed for calibrating the binding energies of the photoelectron. Brunauer-Emmett–Teller (BET) N2 adsorption-desorption analyses were conducted at 77 K using a Micrometrics Surface Area and Porosity instrument (MicroActive for TriStar II 3020 V1.04). The Cu metal content in the Cu@nano-CeO2 nanostructure was assessed through inductively coupled plasma optical emission spectrometry (ICP-OES) analysis on a PerkinElmer Optima 4300DV ICP emission spectrometer. Prior to ICP-OES analysis, each sample underwent complete dissolution in a mixture of HNO3/HCl (1/3; v/v). DPPH radical scavenging assay of Cu@nano-CeO2 The method as described by Blois [35] was applied to assess the antioxidant capability of the Cu@nano-CeO2 based on the scavenging of stable 2,2-diphenyl-1-picrylhydrazyl (DPPH) free radical. While a negative control containing reagents except the sample was used, ascorbic acid and Trolox were used as the positive control. 250 μL different concentrations of sample and controls were transferred into test tubes followed by the addition of 1 mL of DPPH (0.002 %) solution. These test tubes were shaken vigorously and then incubated at room temperature for about 30 min with no light exposure. To determine the inhibition, spectrophotometric analysis at 517 nm was applied to calculate the percentage of free radical scavenging activity (%FRSA). The given following formula was used to compute the FRSA.FRSA(%)=(Abs(control)−Abs(sample)/Abs(control))×100 Effect of Cu@nano-CeO2 on α-amylase activity Various concentrations of the sample at 50, 100 and 200 mg/L were poured into the test tubes. Then phosphate buffer and α-amylase were added and incubated at 37 °C for 15 min. 0.2 mL 2 % potato starch solution was added to initiate the hydrolysis process at 37 °C for 20 min. After the incubation, 0.4 mL 3,5-dinitro salicylic acid (DNS) was added to each test tube to terminate the hydrolysis process. The tubes were then boiled at 100 °C for 5 min. After the mixture cooled, dilution was made using 3 mL distilled water, and spectrophotometric measurements of the mixture were made at 540 nm. The solution without test samples was used as a control. The α-amylase activity was calculated according to the formula below.α−amylaseactivity(%)=(Abs(control)−Abs(sample)/Abs(control))×100 DNA nuclease experiments of Cu@nano-CeO2 The DNA nuclease activity of the Cu@nano-CeO2 was performed using DNA agarose gel electrophoresis studies which is a common laboratory technique used to separate and analyze DNA, RNA, and proteins based on their size and charge. The assays were carried out using pBR322 plasmid DNA. The DNA was treated with increasing concentrations of the sample (50, 100, 200 mg/L) and incubated at 37 °C for 90 min. Then, the 10 × loading buffer was added to the electrophoresis apparatus, and samples were loaded onto an agarose gel (1.0 % w/v) and stained with 0.5 μg/mL EthBr. Electrophoresis was run at 100 V in a Tris-acetic acid-EDTA buffer for 1.5 h. Negative control was applied using untreated plasmid DNA. Finally, the electrophoresis bands were photographed under the UV illuminator. Antimicrobial assays of Cu@nano-CeO2 The standard broth microdilution method was applied. Different bacterial and fungal strains were used for the antimicrobial assay such as three Gram-negative bacteria Escherichia coli (ATCC 25922), Legionella pneumophila subsp. pneumophila (ATCC 33152), and Pseudomonas aeruginosa (ATCC 27853); and three Gram-positive bacteria Enterococcus faecalis (ATCC 29212), Enterococcus hirae (ATCC 10541), and Staphylococcus aureus (ATCC 25923); and two fungus Candida tropicalis (ATCC 750) and Candida albicans. These species were inoculated into a 10 μL aliquot of sterile Nutrient Broth for refreshing and grown at 37 °C overnight before the application. The desired concentration of Cu@nano-CeO2 was poured into the first well of a microplate containing nutrients. Serial dilution of the samples was applied to the other wells. Each well was then inoculated with approximately 1.5 x 108 CFU/mL of microorganisms. During 24 h at 37 °C microplates were incubated on a shaker. In the end, minimum inhibition concentration (MIC) values were determined. Microbial cell viability test of Cu@nano-CeO2 The bacterial cell viability inhibition capacity of Cu@nano-CeO2 was assessed using a model strain E. coli (ATCC 25922). E. coli was grown in an appropriate medium at 37.0 °C for one day using a shaker. Bacterial cells were separated by centrifugation and cleaned with a sterile saline solution to remove the contaminant. Cell viability test was applied after exposing E. coli to varying concentrations of Cu@nano-CeO2 at 37 °C for 2 h. Posttreatment, E. coli inoculated on agar medium and left to incubate for one day at 37 °C. Percentile cell viability was calculated following formula using the ratio of colonies number after exposure to Cu@nano-CeO2 to the non-exposed control one.Microbialcellviability(%)=(Acontrol–Asample/Acontrol)x100 Biofilm inhibition activity of Cu@nano-CeO2 P. aeruginosa and S. aureus overnight culture were diluted in fresh media and adjusted to 1 × 108 CFU/mL. These bacterial suspensions were added to a 48-well plate containing Cu-doped CeO2 concentrations of 12.5, 25, and 50 mg/L. This plate was then incubated at 37 °C for 72 h. To remove planktonic cells, the contents were evacuated and the wells were cleaned three times with distilled water. The bacterial biofilm was stained with 0.1 % crystal violet for 30 min. The surplus dye was washed away with water, then absolute ethanol was used to dissolve the biofilm. The absorbance was measured at 595 nm. The biofilm inhibition was calculated using the formula below.BiofilmInhibition(%)=(Abs(control)−Abs(sample)/Abs(control))×100 Application of polyethersulfone (PES) membrane coated with Cu@nano-CeO2 for E. coli removal and its solid surface antimicrobial activity The application of polyethersulfone (PES) membrane coated with Cu@nano-CeO2 for E. coli removal and its solid surface antimicrobial activity was evaluated according to our previous work [36]. Results and discussion Characterization of Cu@nano-CeO2 nanostructure The structural and morphological properties of the Cu@nano-CeO2 material were evaluated through ICP-OES, XRD, XPS, SEM, and BET analyses. In the initial stage, ICP-OES analysis was employed to assess the distribution of Cu metal content on CeO2 NPs, revealing a Cu content of 1.82 ± 0.06 wt%. It is noteworthy that the designed theoretical metal content of the Cu@nano-CeO2 material was intended to be 2.0 wt% Cu. In the XRD pattern provided in Fig. 1 for determining the crystallinity of nano-CeO2 and Cu@nano-CeO2 samples, it is evaluated that the observed Bragg peaks at 28.5°, 33.2°, 47.5°, 56.3°, 59.1°, 69.5°, 76.7°, 79.2° and 88.6° correspond to the (111), (200), (220), (311), (222), (400), (331), (420), and (422) planes, respectively. When the XRD pattern of nano-CeO2 is compared with the standard diffraction pattern of cerium oxide (JCPDS card number 34–0394), it is observed that the crystal structure of the present cerium oxide sample is cubic fluorite structure [15,33,37,38]. It is also observed that the XRD pattern of Cu@nano-CeO2 completely overlaps with that of nano-CeO2. According to the ICP-OES analysis, no signal for Cu is observed in the XRD pattern due to low Cu doping on the surface of nano-CeO2. However, it is also concluded that there is no alteration or collapse in the crystal structure of nano-CeO2, which is the host material in the nanoparticle production process.Fig. 1XRD patterns of nano-CeO2 and Cu@nano-CeO2 samples.Fig. 1 XRD patterns of nano-CeO2 and Cu@nano-CeO2 samples. XPS offers additional insights into the oxidation state of copper and the surface composition of the resulting Cu@nano-CeO2. In Fig. 2 (a), the survey scan XPS spectrum of the Cu@nano-CeO2 sample illustrates the presence of nano-CeO2 elements (Ce and O) along with copper (Cu). Fig. 2 (b) displays the high-resolution Cu 2p XPS spectrum of the Cu@nano-CeO2 sample, which has a loading of 1.82 ± 0.06 wt% Cu, along with its deconvolution. The deconvolution of the high-resolution Cu 2p XPS spectrum reveals two distinct peaks at 933.2 eV (Cu 2p3/2) and 942.69 eV (Cu 2p1/2), indicating metallic Cu (0), as supported by previous studies [34,39]. Furthermore, peaks observed at 953.21 eV suggest the presence of the CuO phase, likely resulting from the surface oxidation of Cu (0) NPs during the XPS sampling procedure [22,40]. Fig. 2 (c) reveals the high-resolution Ce 3d spectra consisting of spin-orbit pairs Ce 3d5/2 (883.21 eV) and Ce 3d3/2 (900.20 eV). These binding energies are well attributed to the predominant Ce4+ and Ce3+ oxidation states in CeO2 nanoparticles. In the deconvoluted O 1s spectrum (Fig. 2 (d)), the two main binding energies observed at 528.21 eV and ∼528.76 eV can be associated with lattice oxygen ions (Olat) and surface-adsorbed oxygen ions (Oads), respectively [41,42].Fig. 2Survey (a), Cu 2p (b), Ce 3d (c), and O 1s (d) core levels XPS spectra of Cu@nano-CeO2 nanostructure.Fig. 2 Survey (a), Cu 2p (b), Ce 3d (c), and O 1s (d) core levels XPS spectra of Cu@nano-CeO2 nanostructure. The morphological analysis of the Cu@nano-CeO2 nanostructure was conducted using SEM. In Fig. 3(a–c), SEM images of the samples are presented alongside their corresponding EDX spectrum. As depicted in Fig. 3(a and b), Cu NPs exhibit a nearly uniform distribution on the surface of nano-CeO2. Consistent with expectations, the EDX spectra of nano-CeO2 reveal the presence of Ce and O elements alongside carbon, likely originating from the carbon tape used during sample preparation. Additionally, the homogeneous distribution of Cu, Ce, and O observed in the SEM-elemental mapping of Cu@nano-CeO2 (Fig. 3 (d)) further confirms the presence of Cu (0) NPs on the nano-CeO2 support. It is also important to note that the Au signals originate from the SEM sample carrier.Fig. 3SEM images in different scale (a–b), SEM-EDX spectrum (c), and SEM-elemental mapping (d) of Cu@nano-CeO2 nanostructure.Fig. 3 SEM images in different scale (a–b), SEM-EDX spectrum (c), and SEM-elemental mapping (d) of Cu@nano-CeO2 nanostructure. Fig. 4(a–b) displays the N2 adsorption-desorption isotherms for both nano-CeO2 and Cu@nano-CeO2 samples, with BET analysis conducted to assess their surface area and porosity. The isotherms for each sample exhibit type IV and H3 hysteresis loops, in line with the IUPAC classification characteristic of mesoporous materials [43,44]. The BET surface area of nano-CeO2 and Cu@nano-CeO2 was determined as 46.02 m2/g and 38.18 m2/g, respectively, based on the linear portion of the BET plots. The observed decrease in pore volume and BET surface area upon transitioning from nano-CeO2 to Cu@nano-CeO2 can be attributed to the blockage of nano-CeO2 pores by Cu (0) NPs, as evidenced by SEM analysis (as discussed earlier).Fig. 4N2 Adsorption desorption isotherms of nano-CeO2 (a) and Cu@nano-CeO2 (b) samples.Fig. 4 N2 Adsorption desorption isotherms of nano-CeO2 (a) and Cu@nano-CeO2 (b) samples. Free radical scavenging activity (FRSA) of Cu@nano-CeO2 The antioxidant assays assess a sample's antioxidant potential based on its ability to donate electrons or hydrogen atoms [45]. The antioxidant potential of Cu@nano-CeO2 was investigated. The obtained results were evaluated to compare with ascorbic acid and Trolox (Fig. 5). At a concentration of 6.25 mg/L, FRSA of Cu@nano-CeO2, ascorbic acid, and Trolox was 60.73, 72.31, and 74.16 %, respectively. When the concentration was increased up to 100 mg/L, FRSAs was elevated 100 % by Cu@nano-CeO2. It is clearly seen that Cu@nano-CeO2 has significant antioxidant potential depending on the concentration. This antioxidant capability could be attributed to the presence of functional groups on the surface of nanoparticles or to the nanoparticle itself [46]. Because of the two oxidation states of Ce+3 and Ce+4, the free radical scavenging activity of Cu@nano-CeO2 is highly connected to the redox potential [47]. Jan et al. synthesized CeO2 NPs using a green chemistry approach. They also investigated the antioxidant potential of CeO2 NPs and reported that CeO2 NPs showed significant in vitro antioxidant abilities [48]. Butt et al. produced CeO2 NPs via biogenic synthesis. They reported that CeO2 NPs exhibited moderate FRSA (40.6 ± 1 %) [49]. From our findings, we can conclude that the Cu@nano-CeO2 has a strong anti-radical effect.Fig. 5DPPH scavenging activity of Cu@nano-CeO2Fig. 5 DPPH scavenging activity of Cu@nano-CeO2 Enhancement effect of Cu@nano-CeO2 on α-amylase The influence of Cu@nano-CeO2 on the α-amylase enzyme was investigated using the DNS method. As seen in Fig. 6, in a concentration-dependent manner, the tested sample activated α-amylase activity. When the concentration was 50, 100, and 200 mg/L, the promoted ratio reached 293.9, 257.6, and 247.0 %, respectively. Cu NPs in the tested sample structure at a lower concentration significantly enhanced the enzyme activity but gradually decreased with increasing Cu@nano-CeO2 concentration. Similar findings have been reported in the literature for different nanoparticles. Abdel-Nasser et al. reported that the α-amylase activity was increased gradually with increasing the Au and Ag-NPs, but after a certain concentration, enzyme activity was decreased gradually [50]. Saware et al. found that at low concentrations, Ag NPs stimulate α-amylase activity while inhibiting it at high concentrations [51]. According to the data we obtained, amylase activity increased approximately 3 times at 50 mg/L. In this context, Cu@nano-CeO2 can be used to increase α-amylase activity in various industries where α-amylase is used.Fig. 6The effect of Cu@nano-CeO2 concentrations on α-amylase activity.Fig. 6 The effect of Cu@nano-CeO2 concentrations on α-amylase activity. DNA cleavage activity of Cu@nano-CeO2 To investigate the DNA nuclease activity of Cu@nano-CeO2, agarose gel electrophoresis tests were carried out using pBR322 plasmid DNA, as described in the experimental section. When plasmid DNA is treated with a substance capable of breaking the DNA strand, it acts like a nuclease and ‘scissors’ the DNA's supercoiled circular Form I at specific positions to give nicked circular Form II and linear Form III. This was investigated by treating pBR322 plasmid with Cu@nano-CeO2 at 50, 100, and 200 mg/L concentrations. The electrophoresis image is presented in Fig. 7. At 50 mg/L concentration, one strand was cleaved, the supercoiled form I relaxed and relatively slower-moving form II was produced (Lane 2). At 100 and 200 mg/L concentrations of the sample, it was observed that the nuclease activity of Cu@nano-CeO2 was very effective (Lanes 3 and 4) and the complete cleavage of the DNA strand was obtained. In general, 3 different types of DNA cleavage mechanisms can be distinguished, DNA photochemical cleavage, oxidative cleavage, and also hydrolysis, although the first two mechanisms are quite closely related. Probably, Cu@nano-CeO2 compounds caused DNA cleavage via DNA hydrolysis mechanism. The widely accepted mechanism of the DNA hydrolysis reaction is a nucleophilic attack on the DNA phosphate backbone to form a five-coordinate intermediate that can be stabilized by a catalyst. Subsequent cleavage of the 3′-PO or 5′-PO results in strand scission [52]. Consequently, the nuclease experiments applied using agarose gel clearly suggest that the Cu@nano-CeO2 exhibits an effective DNA nuclease activity and Cu@nano-CeO2 can be utilized for anti-cancer and antimicrobial studies.Fig. 7DNA cleavage activity of Cu@nano-CeO2 nanostructure. Lane 1, pBR 322 DNA; Lane 2, pBR 322 DNA +50 mg/L Cu@nano-CeO2; Lane 3, pBR 322 DNA +100 mg/L of Cu@nano-CeO2; Lane 4, pBR 322 DNA +200 mg/L of Cu@nano-CeO2.Fig. 7 DNA cleavage activity of Cu@nano-CeO2 nanostructure. Lane 1, pBR 322 DNA; Lane 2, pBR 322 DNA +50 mg/L Cu@nano-CeO2; Lane 3, pBR 322 DNA +100 mg/L of Cu@nano-CeO2; Lane 4, pBR 322 DNA +200 mg/L of Cu@nano-CeO2. Antimicrobial activity of Cu@nano-CeO2 An antimicrobial assay was performed to determine MIC values of Cu@nano-CeO2 against different microbial strains. MIC values of Cu@nano-CeO2 were 16 mg/L against E. hirae and E. feacalis, 32 mg/L against S. aureus, 64 mg/L against E. coli, 128 mg/L against P. aeruginosa and L. pneumophila subsp. Pneumophila, 256 mg/L against C. tropicalis and C. Albicans (Table 1). The antibacterial mechanism is still unclear, but it is likely proposed as follows. The negatively charged cell walls of both Gram-positive and Gram-negative bacteria electrostatically attract the positively charged Cu@nano-CeO2. Zeta potential (Malvern Zeta Sizer Nano ZS) value of Cu@nano-CeO2 was measured as 2.06 ± 0.13 mV. This interaction cause the release Ce3+, Ce4+ and Cu + ions. These ions induce the production of reactive oxygen species (ROS) on the bacterial cell membrane. ROS generation hinders the antioxidant defense system and damages the cell membrane mechanically [49,53]. Pandiyan et al. fabricated SrO/CeO2 nanostructure using a green synthesis approach. Biofabricated SrO/CeO2 NPs showed important antibacterial activity, especially against S. aureus (G+) than E. coli (G−) bacteria [54]. Maleki et al. synthesized Ag-doped CeO2 NPs using Salvia seeds extract. They reported that Ag-doped CeO2 NPs had excellent antibacterial activity against S. aureus and P. Aeruginosa [53]. The data obtained after antimicrobial activity experiments show that the strong inhibitory effect of Cu@nano-CeO2 is supported by the literature.Table 1Antimicrobial activity of Cu@nano-CeO2Table 1MicroorganismsMICs (mg/L)E. coli64P. aeruginosa128L. pneumophila subsp. pneumophila128E. hirae16E. fecalis16S. aureus32C. tropicalis256C. albicans256 Table 1Antimicrobial activity of Cu@nano-CeO2Table 1MicroorganismsMICs (mg/L)E. coli64P. aeruginosa128L. pneumophila subsp. pneumophila128E. hirae16E. fecalis16S. aureus32C. tropicalis256C. albicans256 Antimicrobial activity of Cu@nano-CeO2 Microbial cell viability ınhibition of Cu@nano-CeO2 The inhibition activity of Cu@nano-CeO2 to E. coli cell viability was evaluated at different concentrations (25, 50, and 100 mg/L). After 2 h of contact with Cu@nano-CeO2, cell viability was determined. The results are presented in Fig. 8. The results indicated that the cell viability of E. coli was strongly inhibited at all tested concentrations by Cu@nano-CeO2. A bacterium's membrane fluidity is essential to maintain a normal cellular structure, cell division, and diffusion functions, and resist environmental stresses [55]. After 2 h of contact between E. coli cells and Cu@nano-CeO2, membrane fluidity may decrease so this was related to the decrease in cell viability. After NPs come into contact with the cell membrane, they enter the cell through interactions such as electrostatic attraction, van der Waals forces, hydrophobic interactions, and receptor–ligand, affecting the shape and function of the cell membrane. Then, NPs interact with the basic components of the microorganism cell, such as lysosomes, DNA, enzymes, and ribosomes, leading to heterogeneous changes, oxidative stress, electrolyte imbalances, changes in cell membrane permeability, enzyme inhibition, gene expression changes, and protein deactivation Wang et al. (2017) [56]. Cu@nano-CeO2 interacts strongly with membrane lipids, which may result in Cu@nano-CeO2 penetration into cell membranes, oxidation of membrane phospholipids by Ce4+, and consequently membrane instability and fluidity reduction [57]. As a result, Cu@nano-CeO2 can be used for effective microbial disinfection.Fig. 8Microbial cell viability inhibition of Cu@nano-CeO2Fig. 8 Microbial cell viability inhibition of Cu@nano-CeO2 Evaluation of antibiofilm activity of Cu@nano-CeO2 Biofilms are classified as self-produced structures by microbes, mainly composed of extracellular polymeric substances such as proteins, carbohydrates, and extracellular DNA. These extracellular polymeric substances enable biofilm stability and aid microbe adhesion to biotic and abiotic surfaces [58,59]. Moreover, the bacteria growing in the biofilms have an inherent resistance to chemical therapeutic drugs like antibiotics. As a result, attacking biofilms is regarded as a novel method of reducing bacterial infections. Cu@nano-CeO2 was tested for anti-biofilm effects against two well-known biofilm-forming bacteria, S. aureus, and P. aeruginosa. Cu@nano-CeO2 exhibited a dose-dependent effect on S. aureus and P. aeruginosa biofilms, as seen in Fig. 9, Fig. 10. At 12.5, 25, and 50 mg/L concentrations of Cu@nano-CeO2, biofilm formation of S. aureus and P. aeruginosa were inhibited at 82.63, 90.13, and 98.27 % and 68.26, 75.49, and 82.14 % respectively, when compared with control. In earlier studies, Altaf et al. reported that biogenic synthesized CeO2 NPs had 70 % inhibition of S. aureus biofilm [60], and Naidi et al. reported 65 % destruction of bacterial biofilm with green synthesized Sn-doped CeO2 NPs [61]. Iqbal et al. reported that biosynthesized CeO2-graphene oxide nanocomposites exhibited 82 and 60 % inhibition of P. aeruginosa and S. aureus biofilm, respectively [62]. Our findings demonstrated that Cu@nano-CeO2 inhibited biofilm production more effectively while also being disruptive to mature biofilm.Fig. 9Biofilm inhibition of S. Aureus.Fig. 9Fig. 10Biofilm inhibition of P. aeruginosa.Fig. 10 Biofilm inhibition of S. Aureus. Biofilm inhibition of P. aeruginosa. Application of polyethersulfone (PES) membrane coated with Cu@nano-CeO2 for E. coli removal and its solid surface antimicrobial activity In order to determine wastewater treatment potential, the inhibition activity of PES/Cu@nano-CeO2 membrane to E. coli cell viability was also investigated. The inhibition activities of bare PES membrane, PES/Cu@nano-CeO2 0.50 wt% membrane, PES/Cu-doped CeO2 1.0 wt% membrane, and PES/Cu-doped CeO2 2.0 wt% membrane were 9.69 %, 37.63 %, 100.0 %, and 100.0 %, respectively (Fig. 11). Moreover, E. coli removal efficiency of the PES/Cu@nano-CeO2 membrane during the wastewater treatment process was tested. For this purpose, the filtrates obtained using the membranes given above were studied for E. coli removal. Obtained results are given in Fig. 12. While bare PES membrane exhibited 10.87 % inhibition activity, PES/Cu@nano-CeO2 0.50, 1.0, and 2.0 wt% membranes exhibited 100.0 % inhibition activity. Our findings demonstrated that the Cu@nano-CeO2 blended membrane has the potential to improve treatment efficiency and water supply by being used in water and wastewater treatment procedures.Fig. 11Performing of PES membrane surface coated with Cu@nano-CeO2 for removal of E. coli. (1: Control; 2: PES Membrane; 3: 0.5 % Cu@nano-CeO2 doped PES Membrane; 4: 1 % Cu@nano-CeO2 doped PES Membrane; 5: 2 % Cu@nano-CeO2 doped PES Membrane.Fig. 11Fig. 12Performing of PES membrane coated with Cu@nano-CeO2 for E. coli filtration process. (1: Control; 2: PES Membrane; 3: 0.5 % Cu@nano-CeO2 doped PES Membrane; 4: 1 % Cu@nano-CeO2 doped PES Membrane; 5: 2 % Cu@nano-CeO2 doped PES Membrane.Fig. 12 Performing of PES membrane surface coated with Cu@nano-CeO2 for removal of E. coli. (1: Control; 2: PES Membrane; 3: 0.5 % Cu@nano-CeO2 doped PES Membrane; 4: 1 % Cu@nano-CeO2 doped PES Membrane; 5: 2 % Cu@nano-CeO2 doped PES Membrane. Performing of PES membrane coated with Cu@nano-CeO2 for E. coli filtration process. (1: Control; 2: PES Membrane; 3: 0.5 % Cu@nano-CeO2 doped PES Membrane; 4: 1 % Cu@nano-CeO2 doped PES Membrane; 5: 2 % Cu@nano-CeO2 doped PES Membrane. Conclusion The Cu@nano-CeO2 nanostructure showed highly potent antioxidant activity as 100 %. It activated the α-amylase enzyme in a concentration-dependent manner and α-amylase enzyme activity was enhanced 293.94 % at 50 mg/L. After nuclease activity experiments using agarose gel, it was determined that Cu@nano-CeO2 nanostructure exhibited an effective DNA nuclease activity. The Cu@nano-CeO2 nanostructure provided highly promising antimicrobial properties and inhibited biofilm formation against S. aureus and P. aeruginosa. The highest biofilm inhibition was determined as 98.3 % against S. aureus. Moreover, it was determined that the Cu@nano-CeO2 nanostructure blended polyethersulfone membrane strongly inhibited E. coli viability (100 %) after it was applied to the wastewater treatment system. CRediT authorship contribution statement Lokman Şener: Methodology, Investigation, Formal analysis, Data curation. Sadin Özdemir: Methodology, Investigation, Formal analysis, Conceptualization. M. Serkan Yalçın: Methodology, Investigation, Formal analysis, Data curation, Conceptualization. Mehmet Gülcan: Writing – review & editing, Writing – original draft, Supervision, Data curation, Conceptualization. Nadir Dizge: Writing – review & editing, Writing – original draft, Supervision, Formal analysis, Data curation. Data availability statement Data will be made available on request. Declaration of competing interest The authors declare the following financial interests/personal relationships which may be considered as potential competing interests: Mehmet Gülcan is an ABM of the Heliyon journal. If there are other authors, they declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.