Hydrogen Trapping at Fe/Cu Interfaces Authors: Philipp Hammer, Matthias Militzer, Vsevolod I Razumovskiy, Salvatore Scirè Published: 2024 ABSTRACT AbstractCopper (Cu) in steel production can be a residual element, causing challenges during steel processing, as well as an alloying element, improving corrosion resistance and providing hardenability by nanosized precipitates. For the transition toward a green economy, increased recycling rates in steel production and alternative energy carriers, such as hydrogen, are of vital importance. As hydrogen is known for its embrittling effect on high-strength steels, this work sought to explore possible mitigation strategies for hydrogen embrittlement (HE) with the help of Cu precipitates. Hydrogen trapping at Cu/Fe interfaces following the complex phase transformations in the Cu precipitation sequence from body-centered cubic (bcc) to the so-called 9R structure to face-centered cubic (fcc) was addressed by a series of systematic density functional theory calculations. In combination with thermodynamic calculations, the pressing question regarding which of the precipitate structures was most desirable for the tackling of HE was alluded to. We found that hydrogen trapping at the Cu/Fe interfaces increased from −0.05 to −0.18 eV following the precipitation sequence. Despite this relatively weak hydrogen trapping, which was in the range of dislocations, we showed through thermodynamic calculations that fcc Cu precipitates could still contribute to lowering the risk of triggering the hydrogen-enhanced localized plasticity (HELP) mechanism of HE.Keywords: hydrogen trapping, interface segregation, DFT calculations, Cu precipitate 1. Introduction Copper (Cu) plays an important role as an alloying element in steel production and can be used to improve the corrosion resistance of various steel grades [1,2,3] or their mechanical properties by nanosized Cu-rich particles [1,4,5,6,7,8]. On the other hand, Cu residuals introduced during the steelmaking process through scrap recycling cannot be easily removed, thus causing challenges during the later stages of steel processing [9,10,11]. The latter effects become increasingly important in view of the green economy, which relies on material recycling and the use of renewable and greenhouse-gas-emission-free energy sources [12,13,14,15]. In terms of recycling, the electric arc furnace (EAF) steelmaking process is of particular interest, which directly uses steel scrap with the aid of electricity as a carbon-free energy source [9,14] but increases the likelihood of Cu residuals in all types of steel grades. In addition, hydrogen (H) is envisioned as one of the most prominent sources of clean renewable energy in the future and the exposure of steel structures to H steadily increases [12,13,14,15]. Unfortunately, the contact between steel and H in service leads to another challenge regarding the safety of high-strength steels known as hydrogen embrittlement (HE) [15,16,17]. A possible implication of a combined effect of H and Cu on steels used in H applications deserves special attention, as it may determine the reliability of high-strength Cu-containing steels in practice [18,19]. One of the most appealing problems in this respect is related to the complex kinetics of precipitate formation in Cu containing body-centered cubic (bcc) steels, which is known to undergo several stages [1,2,6,20,21,22]. During the first stage, Cu forms coherent nanosized particles that inherit the bcc crystal lattice structure of the parent phase (α-Fe). As these particles grow, they transform into the more complex C19 structure with a twinned lattice, also referred to as 9R [2,20,21,22]. In the final stage, Cu precipitates become completely incoherent with the host bcc lattice of iron and adopt the equilibrium face-centered cubic (fcc) structure of Cu. This complex precipitation kinetics is known to have a pronounced effect on the mechanical properties of steels, such as strength, ductility, and fracture toughness, representing a topic of intense investigations [1,2,4,5,6,7,8,21,22]. In the context of HE, coherent precipitates are often used in steel design as traps for H atoms. Such traps can immobilize H atoms, and thus, prevent them from reaching and accumulating at microstructural features critical for HE (like grain boundaries (GBs) and dislocations). H accumulation at and interaction with these features is responsible for triggering either the hydrogen-enhanced decohesion (HEDE) mechanism through H interaction with GBs or the hydrogen-enhanced localized plasticity (HELP) mechanism via H interplay with dislocations. Both of these mechanisms are regarded to be among the most prominent for high-strength steels [15,23,24]. A key factor influencing the efficacy of traps to immobilize H is their trapping energy, i.e., the interaction energy of H with the trapping site, which determines how strongly H is bound to the trap. Another important metric is the amount of H traps that can be provided by such precipitates, as they are only effective in their role as long as they are not saturated with H [25]. This concept has been known for the case of coherent transition metal carbide precipitates in low-alloyed steels [15,16,25,26,27,28,29,30,31], whereas much less is known about the possible role of Cu precipitates in this process, though there are indications in the literature that some Cu precipitates may play a similar role to carbides in terms of H trapping [32,33,34,35,36,37,38,39,40,41,42,43,44]. The main reason for the limited data on H interaction with Cu nano-precipitates is related to the technical difficulties of experimental studies and theoretical description. On the experimental side, the detection of both H atoms and nano-precipitates is often found at the limits of sensitivity or resolution for modern experimental methods of microstructure characterization, making it necessary to apply multiple methods at a time to obtain a conclusive answer [45]. This makes the direct observation of H interaction with microstructural features at the nanoscale an extremely challenging task. On the computational side, the complexity of the twinned 9R structure with a nine-layer-repeated stacking sequence for Cu precipitates (see Section 2.2.3 for details) poses particular challenges for predictive density functional theory (DFT) calculations, as the necessarily large supercells used to describe this structure are at the limits of computational feasibility. In this study, we analyzed H interactions with Cu particles in bcc iron using DFT and thermodynamic modeling. First, we constructed atomic scale interface models following crystallographic and high-resolution TEM data for three types of Cu precipitates in iron, i.e., bcc, fcc, and the 9R twinned lattice with a nine-layer-repeated stacking sequence. These models were used to determine the H-trapping energies by DFT. As a final step of our investigation, we employed these DFT results to simulate possible redistributions of H within a typical microstructure of a high-strength martensitic steel containing Cu precipitates using a thermodynamic model of H trapping. A parameter study on the influence of Cu precipitate shape and volume fractions on H redistribution closed this study, where Cu precipitate contents that stemmed from residual levels of Cu up to Cu as a deliberate alloying element in steel were considered. The findings of this investigation were used to elaborate on how one challenge of the green economy, that is, increased levels of unwanted Cu residuals due to scrap recycling, provides a possible mitigation strategy for the HE problem that is anticipated to become larger in the wake of the green energy transition. 2. Computational Details 2.1. DFT Calculations First-principles density functional theory (DFT) calculations were performed with the Vienna ab initio simulation package (VASP, version 5.4.4) [46,47,48] using the Perdew, Burke, and Ernzerhof [49] description of the generalized gradient approximation (GGA) for the exchange–correlation functional. The valence electron configurations for the atomic potentials based on the projector-augmented wave (PAW) [50,51] method were 3p64s13d10 for Cu, 3p64s23d6 for Fe, and 1s1 for H. For all calculations, a plane-wave energy cutoff of 400 eV and spin polarization were employed and electronic self-consistency was converged to 10−7 eV/atom for the total energy. Unless stated otherwise, ionic relaxations with constant cell shape and volume were undertaken until the residual forces reached 0.02 eV/Å per atom. Electronic smearing was considered using the Methfessel–Paxton method [52], with a width of 0.2 eV to improve the convergence. The Monkhorst–Pack [53] grid sampling for Brillouin zone integration was automatized by the pymatgen [54] software package (version 2022.3.29), with the reciprocal k-point density set to 1200 Å−3. The equations of state were calculated using the Birch–Murnaghan [55] fit to the energy versus volume curves obtained by a homogeneous distribution of seven points ±15% around the minimum energy volume from Ref. [56]. Based on this fit, the equilibrium lattice parameters for Cufcc, Cubcc, and Febcc were determined as 3.635 Å, 2.890 Å, and 2.838 Å, respectively. Our results were found to be in good agreement with the existing literature reporting lattice parameters of 3.63 Å [57,58] for Cufcc, 2.888 Å [59] for Cub cc, and 2.831 Å [60] to 2.84 Å [61] for Febcc. The H solution energy in the tetrahedral interstitial site of Febcc was previously determined by the authors [26] as 0.21 eV, comparing well with the values of 0.21 eV [62] and 0.23 eV [60] determined in the literature. In the same way, H solution energies in Cu were calculated, which resulted in 0.43 eV and 0.54 eV for the octahedral and tetrahedral interstitial sites in Cubcc, as well as 0.45 eV and 0.65 eV for the octahedral and tetrahedral interstitial sites in Cufcc, respectively. Our result for the octahedral interstitial site in Cufcc aligns with the experimentally determined H solution energy of 0.44 eV [63], as well as the value of 0.41 eV [58] obtained by DFT calculations. 2.2. Interface Models Coherent interfaces between the Fe matrix and Cu precipitates were modeled using slabs with Born–Von Kármán [64] periodic boundary conditions and a vacuum layer in the direction perpendicular to the interface. The assumption that the lattice of the softer (bulk modulus Bm of Cufcc: 139 GPa, Cubcc: 137 GPa) coherent nanosized Cu precipitates adopts the lattice parameter of the stiffer (Bm = 180 GPa) Fe matrix was used for the construction of all interfaces [22,59,65,66,67] and was achieved with the aid of the atomic simulation environment (ASE) [68]. All interface slabs contained a vacuum layer of 20 Å for the cases of bcc and fcc Cu precipitates and 10 Å for the reduced 9R interface. Structure visualizations were carried out using VESTA (version 3.5.5) [69] software and the POSCAR files are provided in the Supplementary Materials. 2.2.1. Cubcc/Febcc Interface In the initial precipitation stage, Cu precipitates adopt the structure of the Febcc matrix phase [22,59,65,66,70,71]. The most commonly assumed orientation relationship (OR) for the corresponding interface is 001Cu ‖ 001Fe with 100Cu ‖ 100Fe [59]. However, the recent study of Garret and Race [66] showed that the high-energy 001Cu ‖ 001Fe interface makes up no more than 20% of the total interface area for precipitates < 5 nm. Instead, TEM investigations [22,65,70,71,72] confirmed that the 011Cu ‖ 011Fe interface dominates for coherent Cubcc precipitates, as it displays the smallest interface energy [66,67]. In this study, we considered both aforementioned cases, i.e., the 001Cu ‖ 001Fe with 100Cu ‖ 100Fe OR and 011Cu ‖ 011Fe with 111¯Cu ‖ 111¯Fe OR, as shown in Figure 1a,b. Atomic structure of (a) the 001Cu ‖ 001Fe interface with Cubcc, (b) the 011Cu ‖ 011Fe interface with Cubcc, and (c) the 111Cu ‖ 011Fe Kurdjumov–Sachs interface with Cufcc. The Cu slabs (orange atoms) are stacked on top of the Fe slabs (grey atoms). The H positions investigated for later trapping energy calculations are marked with green atoms and red atoms, representing H initially placed in sites with tetrahedral and octahedral symmetries, respectively. In the case of the 001Cu ‖ 001Fe interface, slabs that consisted of 3×3×5 repetitions of the respective Febcc and Cubcc unit cells were stacked on top of each other, with 100Fe and 100Cu oriented in the x-direction and 010Fe and 010Cu in the y-direction. The resulting interface cell displayed a lateral size of 8.51 Å in both directions and 10 layers of Fe (grey) and Cu (orange) atoms (180 total atoms), as can be seen in Figure 1a, with the Cu slab compressed by where a100Febcc and a100Cubcc are the lattice spacings of bcc Fe and bcc Cu in their respective 100 directions. The 011Cu ‖ 011Fe interface shown in Figure 1b was constructed by stacking 3×1×5 repetitions of the Febcc and Cubcc slabs with 111¯Fe and 111¯Cu aligned in the x-direction and 2¯11¯Fe and 2¯11¯Cu in the y-direction, respectively. In this process, the Cu slab was compressed by −1.80% in the 111¯-direction and −1.81% in the 2¯11¯-direction to match the respective lateral cell vectors of 7.373 Å and 6.951 Å for Fe. The direction perpendicular to the interface consisted of 10 layers of both Fe and Cu, which resulted in a total number of 180 atoms for the interface cell. 2.2.2. Cufcc/Febcc Interface Cu adopts its native fcc structure at the final stage of precipitation, forming the Kurdjumov–Sachs (K-S) OR with the Febcc matrix: 11¯1Cu ‖ 011Fe with 110Cu ‖ 11¯1Fe [40,73,74]. This interface was constructed using 1×3×2 repetitions of the Cufcc slab with 101¯Cu aligned in the x-direction and 1¯21¯Cu alongside the y-direction, which were stacked on top of 1×2×3 times the Febcc slab, using 111¯Fe as the x-axis and 2¯11¯Fe as the y-axis, as shown in Figure 1c. Therefore, the Cu side of the slab was compressed by −4.40% in the 101¯Cu-direction and elongated by 4.09% in the 1¯21¯Cu-direction. The resulting slab had a total of 72 atoms distributed over 6 Cu and 6 Fe layers and a cell size of 2.458×13.903×42.534Å3. 2.2.3. Cu9R/Febcc Interface In the precipitation sequence αsupeRsatuRated→Cubcc→Cu9R→Cufcc [4,5,22,74], the initial Cubcc precipitates undergo a martensitic transformation into the 9R structure once they reach a critical size of approximately 4 to 9 nm in diameter [4,21,22,75,76,77]. The bulk unit cell of the 9R structure can be idealized as orthorhombic, with lattice constants a, b, and c, although more strictly, it is reported as monoclinic, showing an angle β0 between the base plane and the c-axis slightly different from 90° [22,75,76,77,78]. The three close-packed planes A, B, and C shown in Figure 2a are the building blocks of the 9R unit cell, with the stacking sequence ABC/BCA/CAB shown in Figure 2b,c [70,75,77,78]. The 9R structure can thus be considered an intermediary between the ABC/ABC stacking for fcc and the AB/AB stacking for hexagonal close-packed (hcp) structures, resulting in stacking faults after three close-packed planes, as marked with an underline in the stacking sequence above and with blue planes in Figure 2b,c [22,70,75,78]. A complete relaxation of this structure in DFT yielded a = 4.40 Å, b = 2.54 Å, and c = 18.70 Å, consistent with earlier experimental observations [20,76] of a = 4.33 Å, b = 2.50 Å, and c = 18.36 Å. Schematic representation of the 9R structure, showing (a) the atom positions in relation to the cell parameters a, b, and c on the three close-packed planes (A, B, C) from the top view and the stacking sequence in the (b) front and (c) isometric views [70,75,76,78]. The stacking faults are marked by blue planes in (b,c) [70]. The 9R precipitate forms an interface with the Febcc following the 114¯9R ‖ 011Fe and 1¯109R ‖ 11¯1Fe ORs [20,21,22,65,71,75,76,78,79]. Construction of this interface at the atomic level is not as trivial as in the case of the Cubcc/Febcc and Cufcc/Febcc interfaces described earlier. Thus, the following procedure [77] was employed to construct the Cu9R/Febcc interface with 114¯9R ‖ 011Fe and 1¯109R ‖ 11¯1Fe ORs. First, two vectors that define the 114¯9R plane were identified as −10−1/49RT and −1109RT, as the plane intercepted the cell axis at 1·a, 1·b, and −1/4·c. The vector perpendicular to these two vectors, and thus, normal to the 114¯9R plane, was determined by their cross-product following Equation (2). We named this vector zcart, as it defines the z-direction of the Cu9R slab and it needs to be calculated in the Cartesian rather than 9R-space for the cross-product to be valid. Consequently, each fractional vector in 9R-space has to be multiplied by the matrix of cell parameters C=a000b000c9R. To convert zcart back into 9R-coordinates, Equation (3) is solved for z9R. Finally, z9R can be normalized into a more convenient form using Equation (4): where the superscripts x, y, and z denote the individual vector components in the respective axis directions. Similarly, assuming the direction given in the orientation relationship (1¯109R) will be the x-axis of the cell, the y-axis can be calculated from the cross-product of the calculated z-axis and the x-axis, again in Cartesian coordinates (Equations (5)–(7)). Using the aforementioned calculated lattice parameters for the Cu9R unit cell of a = 4.40 Å, b = 2.54 Å, and c = 18.70 Å, the Cu9R slab was defined by the base vectors of x9RT=1¯109R, y9RT=12.991.009R≈1319R, and z9RT=4.52013.521¯9R≈9272¯9R. This slab contained 396 Cu atoms, was fully repeatable in all dimensions, and aligned the 114¯9R plane and the 1¯109R-direction along the z- and x-axes, respectively. The iron slab with 11¯1Fe was aligned in the x-direction, 211¯Fe in the y-direction, and 011Fe in the z-direction could be straightforwardly generated from the bulk of Febcc, and 2×3×4 repetitions of it were combined with the Cu9R slab to generate the interface, as shown in Figure 3a,b. Thereby, Cu9R was compressed by −3.24% in the 1¯109R-direction and elongated by 1.11% in the 1319R-direction to produce an interface cell with a size of 4.915×20.854×78.121Å3, 8 layers (144 atoms) of Fe, and 22 layers (396 atoms) of Cu. Due to its size and number of atoms, direct DFT calculations for this interface were computationally very demanding. For the hydrogen-trapping calculations, it was thus truncated in the z-direction down to seven layers on each side of the interface, i.e., 126 atoms each for Fe and Cu, with a total of 10 Å of vacuum, as shown in Figure 3c. Atomic structure of the 114¯9R ‖ 011Fe interface using the fully repeatable Cu9R slab in (a) isometric and (b) front views. The figure in (c) details the highlighted section from (b), showing an interface cell using only seven layers of Cu and Fe and outlining the size of a Cu9R unit cell, although the stacking sequence started at a C layer for convenience. Stacking fault planes [70] and the investigated H position are marked in (c) with blue dashed lines and a green atom, respectively. The size of the Cu9R unit cell is indicated by a dashed box in (c). 2.3. Hydrogen-Trapping Energy The H-trapping energy Etp for a position p at a Cu interface with Fe is defined as follows [25,26,27,60]: where EHp[nFe;nCu;1H] and E0p[nFe;nCu] are the total energies of supercells with and without H in the trapping position p, respectively, and containing a number of nFe and nCu atoms. The total energies of a 4×4×4 (128 atom) Febcc supercell with and without H in the tetrahedral interstitial site are denoted as EHFebulk[128Fe;1H] and E0FEbulk[128Fe] and define the reference state for H [26]. By the definition of Equation (8), Etp<0 indicates that H prefers the position in trap p over the tetrahedral interstitial site in Febcc. 2.4. Thermodynamic Model Oriani [80] proposed a thermodynamic model to describe equilibrium H redistribution between the interstitial lattice sites and the available trap sites, depending on their amount (N) and the strength of H trapping (Et). Over recent decades, this model was extended and generalized by a number of authors [25,81,82,83]. Here, we used the most recent version of it, as described in Refs. [25,83] in detail. This thermodynamic model assumes that each unit volume element of a material contains Nti moles of trap types i=1,...,m and NL moles of interstitial lattice sites accessible for H atoms. Mass balance necessitates that the total H concentration cH in the system is equal to the sum of the lattice concentration cL and trap concentrations cti. The fractional occupations (0≤y≤1) of the lattice and trap sites are defined as the H concentration in those sites divided by the total number of available sites and reads as yL=cL/NL and yti=cti/Nti, respectively. With these considerations and the definition that Et<0 is required for H trapping, the original Oriani [80] equation becomes [25,81,83] where Eti is the H-trapping energy of trap i, R is the ideal gas constant, T the absolute temperature, and Ki the equilibrium constant for trap occupation. Re-writing Equation (9) in terms of concentrations and considering mass balance leads to a set of equations such that which can be solved iteratively for the lattice (cL) and trap concentrations (cti), given the total H concentration cH, the trapping energy (Eti), and the number (Nti) of traps of type i. The SciPy [84] software package (version 1.8.0) for Python was used to solve Equation (10). The trap densities (number of available trap sites Nti) of the most common traps, i.e., dislocations, grain boundaries, and precipitates, can be deduced from experimental microstructure characterization data, as outlined by Turk et al. [85]. According to their work, the trap density due to dislocations Ndisl scales with the dislocation density ρ according to where NL is the lattice trap density of 2.04×105 mol/m3 [81,85] and b is the magnitude of the Burgers vector (2.5×10−10 m [85]). The grain boundary trap density can be estimated by the average grain diameter dg following with NA representing Avogadro’s number. Likewise, the trap density associated with precipitate interfaces can be calculated using [86] where A, V, and fV are the precipitate interface area, volume, and volume fraction, respectively. Thus, Equation (13) can be reduced to [86] for spherical precipitates with diameter dprec (A=dprec2π, V=dprec3π6). 3. Results 3.1. Hydrogen Trapping at Cu/Fe Interfaces from DFT The H-trapping energies at the different Cu/Fe interfaces were obtained by placing a H atom at selected interstitial interface positions p with tetrahedral (green atoms) or octahedral (red atoms) symmetry and having at least one Cu and one Fe atom as the nearest neighbors (see Figure 1 and Figure 3). The trapping energies for all the investigated H positions are summarized in Figure 4. Bars in the figure mark the lowest trapping energy, i.e., the deepest trap position, found for a specific interface. For each interface, squares and triangles display the values calculated for H initially placed in positions with octahedral or tetrahedral symmetry, respectively. The alignment of the data points with respect to the bars was connected to the H position on the interface, where the left edge of each bar represents the position of the first Cu layer, while the right edge marks the first Fe layer. H-trapping energies at various Febcc/Cu interfaces ordered according to the Cu precipitate crystal structure and precipitation sequence. The bars display the lowest trapping energy for each interface, and the individual values for each investigated H position are represented by triangles and squares for H initially placed in sites with tetrahedral and octahedral symmetries, respectively. For the Cubcc(0 0 1) ‖ Febcc(0 0 1) and Cubcc(0 1 1) ‖ Febcc(0 1 1) interfaces, the interstitial positions for H were straightforward to determine due to the continued bcc stacking in the supercells, as shown in Figure 1a and Figure 1b, respectively. Figure 4 illustrates that the high-energy Cubcc(0 0 1) ‖ Febcc(0 0 1) interface exhibited two positions capable of moderate H trapping. With a trapping energy of −0.29 eV, the most favored H position at this interface was one with H initially placed in a tetrahedral site at the level of the first Fe layer. In contrast, the low-energy Cubcc(0 1 1) ‖ Febcc(0 1 1) interface displayed almost no H-trapping capability, where three positions of various symmetries showed almost the same trapping energy of −0.05 eV. All tetrahedral or octahedral interstitial positions considered for H trapping at the Cufcc(0 1 1) ‖ Febcc(0 1 1) K-S interface are shown in Figure 1c. There was a total of 13 octahedral and 18 tetrahedral non-equivalent positions that were calculated using DFT. The results show an energy range from close to zero down to −0.18 eV. As in the case of the Cubcc ‖ Febcc interface, the lowest trapping energy was shared by multiple H positions with both initial octahedral or tetrahedral symmetries. The investigated Cu9R1 1 4¯ ‖ Febcc(0 1 1) interface simulation cell that consisted of 252 atoms is displayed in Figure 3c. Here, we placed a H atom at the interstitial interface position with the largest Voronoi volume within the pre-relaxed interface structure. The considered H position is shown in Figure 3c, where it lies between the B layer of the Cu9R slab and a stacking fault plane (A layer). The calculated H-trapping energy for this interface was −0.15 eV, which is comparable to that of the most potent trapping sites (−0.18 eV) at the interface of fcc Cu precipitates. 3.2. Thermodynamic Modeling of Hydrogen Trapping at Cu/Fe Interfaces Required input parameters for modeling the equilibrium H concentration at crystal lattice defects are the total H concentration cH, absolute temperature T, H-trapping energies Eti at all types of considered crystal lattice defects (i), and the corresponding trap densities Nti. In the model calculations, we assumed a total H concentration of 1 wt.ppm and room temperature of 293.15 K (20 °C). The trap densities were estimated based on a high-strength martensitic steel with 1.3 wt.-% Cu from Ref. [7] that had the following defects (traps): dislocations, prior austenite grain boundaries (PAGBs), and Cu precipitates. Hot-rolled samples of this steel were solution-treated at 900 °C for 50 min, water-quenched, and then aged at 525 °C for 25 h, which resulted in an ultimate tensile strength of 950 MPa, and thus, a potential susceptibility to HE in the service condition, i.e., at room temperature [7]. After the heat treatment, a prior austenite grain size of 14.8 μm, a dislocation density of 4.8×1014 m−2, and 1.6 vol.-% of Cu precipitates with an equivalent circle radius of ≈5 nm (dCu≈ 10 nm) were determined [7]. As reported in Ref. [79], fcc Cu precipitates retain a spherical shape immediately after de-twinning from the 9R structure and grow into a rod-like shape with prolonged tempering. For the sake of comparing the influence of different precipitate shapes, we first approximated the Cu precipitates with a spherical shape of the reported equivalent radius, although the actual precipitate shape was described as rod-like with a radius of ≈3.2 nm and length of ≈20 nm [7], which is elaborated on in Section 4. No mention of the precipitate structure was made in Ref. [7], but considering the precipitate shape and comparing the reported precipitate size of ≈20 nm on the long axis with the critical size for the Cu9R→Cufcc transformation (≈12–13 nm [22], 12–20 nm [6]), the Cu precipitates can reasonably be assumed to be fcc type. We therefore chose the minimum H-trapping energy of −0.18 eV—as calculated for the Cufcc ‖ Febcc interface—as the model parameter for the Cu precipitates. Please note that the estimated H concentration values for Cu precipitates represent the maximum concentration, as they were based on the minimum trapping energy value. The trapping energies at dislocations and PAGBs were taken from Sato and Takai [87], who rigorously determined the de-trapping activation energies (Ea) by cryogenic thermal desorption spectroscopy. They are related to the trapping energies (Et) required as input via the Kirchheim criterion Ea≅Emig−Et [25,27,88,89], with the migration barrier Emig of 0.09 eV (8.68 kJ/mol) [25,26,27,90]. The trap densities for dislocations, PAGBs, and Cu precipitates could be estimated by Equations (11)–(14) using the microstructural parameters obtained by Ref. [7]. The absolute values of all input parameters used for the thermodynamic modeling of H trapping in a high-strength martensitic steel with Cu precipitates [7] are summarized in Table 1. Table 1Input parameters for the thermodynamic model.ParameterValueReferenceComment cH 1 wt.ppm-Model assumption T 293.15 K-Room temperature (20 °C) Etdisl. −19.9 kJ/mol[87]8.68 kJ/mol migration barrier [25,26,27,90] −Ea EtGB −35.0 kJ/mol[87]8.68 kJ/mol migration barrier [25,26,27,90] −Ea EtCufcc −17.4 kJ/mol Table 2 −0.18 eV converted to kJ/mol ρ 4.8×1014 m−2[7]Martensite tempered at 525 °C for 25 h dg 14.8 μm[7]Martensite tempered at 525 °C for 25 h dCu 10 nm[7]Martensite tempered at 525 °C for 25 h fCu 1.6 vol.-%[7]Martensite tempered at 525 °C for 25 h Nl 2.04×105 mol/m3[81,85]Lattice trap density for ferrite Ndisl 4.81×102 mol/m3Equation (11)Dislocation trap density NGB 5.39 mol/m3Equation (12)Grain boundary trap density NCu 2.55×102 mol/m3Equation (14)Trap density of Cufcc precipitates Input parameters for the thermodynamic model. Model calculations for the equilibrium distribution of 1 wt.ppm H were conducted with and without Cu precipitates to investigate their potential impacts on the H redistribution, as represented by opaque and transparent bars in Figure 5, respectively. In the original state, H primarily occupied positions at PAGBs (0.53 wt.ppm) and dislocations (0.42 wt.ppm). With the introduction of spherical (dCu = 10 nm) fcc Cu precipitates, the equilibrium H concentration at all other sites was lowered to 0.07 wt.ppm H accumulated at the Cufcc ‖ Febcc interface (see Figure 5a). The majority of this H was redistributed from dislocations, which reduced the H amount bound at dislocations by 11.6%. In addition, 3.0% and 11.7% of H from PAGBs and the lattice were drawn to the fcc Cu precipitates. Redistribution of 1 wt.ppm H among common traps in the high-strength martensitic steel with 1.3 wt.-% Cu [7]. Transparency of the bars represents the reduction in H content due to the formation of Cu precipitates (i.e., the original H content without Cu precipitates prior to redistribution). The input parameters were taken from Table 1. 4. Discussion The results of our DFT calculations show that the Cubcc(0 0 1) ‖ Febcc(0 0 1) interface provided the strongest traps (Et = −0.29 eV) of all the considered interfaces, including bcc, 9R, and fcc types. However, Garret and Race [66] showed that this relatively high energy interface accounted for less than 20% of the Cubcc precipitate interface area or even may not occur at all. The authors suggest that it is rather the Cubcc(0 1 1) ‖ Febcc(0 1 1) interface that dominates for Cubcc [66] precipitates in iron. Our results show, however, that this interface was much less relevant for H trapping due to its negligibly small trapping energy of −0.05 eV. Experimental observations [22,65,70,71,72] suggest that the Cu precipitates of all types predominantly form their interfaces with the (0 1 1) plane of Febcc. The H-trapping energies of −0.05 eV, −0.15 eV, and −0.18 eV calculated at these interfaces follow the precipitation sequence Cubcc→Cu9R→Cufcc [4,5,22,74], respectively (see also Figure 4). These trapping energies fall in a similar range to those of dislocations in Febcc, and thus, are significantly weaker than the H-trapping energies at GBs and vacancies (see Table 2) [60]. This result implies that Cu precipitates of all types do not represent strong traps for H atoms, i.e., they may release H at close-to-ambient conditions [25]. The similarity of the corresponding trapping energies to dislocations would also suggest that it may be difficult to experimentally distinguish H trapping at these precipitates from other defects. Table 2Comparison of the H-trapping energies at Cu/Febcc(0 1 1) interfaces with trapping data on other defects in Fe [60]. Cubcc/FeCu9R/FeCufcc/FeDislocationGBVacancyEt [eV] −0.05−0.15−0.18−0.2–−0.3 [60]−0.18–−0.61 [60]−0.5–−0.7 [60] Comparison of the H-trapping energies at Cu/Febcc(0 1 1) interfaces with trapping data on other defects in Fe [60]. Despite their relatively low trapping energy, Cu precipitates may still have an important role in the distribution of H within a steel microstructure. As is evident from Equation (10), not only the trapping energy but also the trap density affect the H distribution [25,80,81,83]. The model results presented in Figure 5 show that H is expected to be mostly concentrated at dislocations and PAGBs in the martensitic high-strength steel from Ref. [7], where it is known to be the most critical for the HE sensitivity, triggering the HELP and HEDE mechanisms of HE, respectively [15,16,17,24,25]. A total of 1.6 vol.-% Cufcc precipitates with a 10 nm diameter could substantially reduce the concentration of H at dislocations by introducing relatively large amounts of new traps. This microstructural change corresponded to a H concentration drop of 11.6% (from 0.42 wt.ppm to 0.37 wt.ppm) at dislocations and 11.7% at interstitial lattice sites, which reduced the potential effect of the HELP mechanism of HE in this alloy. The above example considers spherical Cufcc precipitates as the major Cu precipitate type that traps H in the model. However, Cu9R precipitates provide a much larger interface area than Cufcc precipitates owing to their smaller size of d9R≈ 5 nm [22]. Additionally, their trapping energy (−0.15 eV = −14.5 kJ/mol) is only little smaller than that of Cufcc, and hence, a larger effect on hydrogen trapping would be expected. Although the provided trap density by Cu9R precipitates (N9R = 5.1×102 mol/m³) is indeed almost double that for Cufcc precipitates (see Table 1), their slightly smaller trapping energy interestingly still caused overall less efficient H trapping. This is illustrated by the leftmost bars in Figure 6, calculated for Cu9R precipitates that were assumed to have a spherical shape of diameter d9R = 5 nm and the same volume fraction as for the Cufcc precipitates (1.6 vol.-%). The dotted line above the bars represents the results of spherical Cufcc from Figure 5, and the shaded area is the original H concentration without Cu precipitates. Redistribution of 1 wt.ppm H among common traps in a high-strength martensitic steel with different types of Cu precipitates [7]. For each trap, the bars from left to right represent 1.6 vol.-% spherical 9R Cu precipitates with a diameter of 5 nm (filled bar) and rod-shaped fcc Cu precipitates with a diameter of 6.4 nm; a height of 20 nm; and volume fractions of 0.5 vol.-% (striped pattern), 1.6 vol.-% (checkerboard pattern), and 2.5 vol.-% (caro pattern). Transparent bars represent the original H content without Cu precipitates and the dotted lines mark the results for spherical fcc Cu precipitates with a diameter of 10 nm (see Table 1) for comparison. Conversely, Cufcc precipitates are reported to have elliptical [22] or rod-like shapes [7] rather than a spherical one. The use of the effective sphere radius to estimate the precipitate trapping served as a first approximation, as a sphere displays the lowest possible surface-to-volume ratio. When approximating the rod-like Cufcc precipitate as a cylinder with a diameter of 6.4 nm and a height of 20 nm [7]—which corresponded to the 10 nm equivalent spherical diameter [7] in Table 1—the trap density calculated according to Equation (13) increased to NCu,rod = 3.08×102 mol/m³. This led to an increased H concentration trapped at Cufcc precipitates, as depicted by the bars with a checkerboard pattern for all traps in Figure 6. In addition, the volume fraction of the Cu precipitates, and thus, their contribution to H trapping, could vary due to a decreased or increased Cu content in the steel. We showcase the effect of the precipitate volume fraction on H trapping in Figure 6 by considering volume fractions of 0.5 and 2.5 vol.-% of rod-shaped Cufcc precipitates with the aforementioned dimensions, as represented by the second and fourth bars with striped and caro patterns, respectively. Thus, an increased volume fraction of 2.5 vol.-% of rod-shaped fcc Cu precipitates could reduce the respective amount of H trapped at dislocations and prior austenite grain boundaries by 19.4% and 5.3% from the original concentration without Cu precipitation. In contrast, 0.5 vol.-% or less of Cu precipitates, which could be introduced by Cu residuals in the steel, only showed a minor effect on the overall H distribution. The overall theoretical results and conclusions are supported by the earlier experimental studies of Komazaki, Koyama, and Misawa [36] and McCarroll et al. [37]. Based on atom probe tomography (APT) results on deuterium-charged samples, McCarroll et al. [37] established a trapping ranking in their steel of TiC-decorated dislocations > high-energy grain boundaries > low-energy grain boundaries > Cu precipitates, emphasizing the rather weak H trapping at Cu precipitates. A similar result was obtained by Lin et al. [38], who determined a ranking of H traps in Cu-containing steel as TiC > TiC platelets > grain boundaries > ε-copper precipitates > dislocations, similar to our results. Komazaki, Koyama, and Misawa [36] found that the fcc-structured ϵ-Cu precipitates showed a better performance than the Cu clusters/twinned 9R precipitates in a small punch test with H contents from 0.75–1.66 wt.ppm, supporting our conclusions. Other similar studies often contained a mixed ferritic/austenitic matrix [33,34,35] or substantial amounts of other precipitate-forming elements, like Ti [36,37,38], Nb [39,40,41], V [41,42], Cr [37,39,40,43], or Mo [38,41,43], providing additional H traps, and thus, making it difficult to single out the effects of Cu precipitates and their morphology on H trapping or HE in these alloys, and therefore, they were not used for comparison with the model results presented here. 5. Conclusions In this study, thermodynamic simulations to determine the H distribution and concentration at individual crystal lattice defects were conducted in order to determine the possible impact of Cu precipitates on the HE susceptibility of a selected steel microstructure. The input parameters were obtained from DFT calculations of the H-trapping energies at model Cu/Fe interfaces with different morphologies, and estimates of the corresponding trap densities were obtained from experimental input of Ref. [7]. The main conclusions are as follows: Despite relatively low absolute values of H-trapping energies, Cufcc precipitates with a large interface area could markedly reduce the amount of H at dislocations, which lowers the risk of triggering the HELP mechanism of HE [15,24]. Despite relatively low absolute values of H-trapping energies, Cufcc precipitates with a large interface area could markedly reduce the amount of H at dislocations, which lowers the risk of triggering the HELP mechanism of HE [15,24]. The H-trapping energy obtained by the DFT calculations follows the experimentally observed evolution of the Cu precipitate structure αsupersaturated→Cubcc→Cu9R→Cufcc [4,5,22,74], with trapping energies of −0.05 eV, −0.15 eV, and −0.18 eV for the model interfaces of Cubcc, Cu9R, and Cufcc precipitates with Fe, respectively. These results are found to agree well with the experimental findings of Refs. [36,37,38,41]. The H-trapping energy obtained by the DFT calculations follows the experimentally observed evolution of the Cu precipitate structure αsupersaturated→Cubcc→Cu9R→Cufcc [4,5,22,74], with trapping energies of −0.05 eV, −0.15 eV, and −0.18 eV for the model interfaces of Cubcc, Cu9R, and Cufcc precipitates with Fe, respectively. These results are found to agree well with the experimental findings of Refs. [36,37,38,41]. The strongest trapping energy of −0.18 eV obtained for the Cufcc/Fe interface is found to be in the range of dislocations, and thus, is considered rather moderate compared with GBs, vacancies, and interfaces with coherent carbides, which all have significantly lower trapping energies (i.e., are stronger traps) for H atoms in Febcc [25,60]. The strongest trapping energy of −0.18 eV obtained for the Cufcc/Fe interface is found to be in the range of dislocations, and thus, is considered rather moderate compared with GBs, vacancies, and interfaces with coherent carbides, which all have significantly lower trapping energies (i.e., are stronger traps) for H atoms in Febcc [25,60]. Although the Cu9R precipitates provide a substantially increased trap density compared with the Cufcc precipitates due to their smaller size, the Cufcc precipitates could still trap a higher concentration of H owing to them offering slightly deeper traps. This emphasizes the importance of trapping energy differences even as small as 3 kJ/mol on the trapped concentration of H for weak-to-moderate H traps. Although the Cu9R precipitates provide a substantially increased trap density compared with the Cufcc precipitates due to their smaller size, the Cufcc precipitates could still trap a higher concentration of H owing to them offering slightly deeper traps. This emphasizes the importance of trapping energy differences even as small as 3 kJ/mol on the trapped concentration of H for weak-to-moderate H traps. While Cufcc precipitates with a large interface area introduced through intentional Cu alloying might significantly contribute to the H redistribution in a steel microstructure, Cu residuals from the steelmaking process are expected to only have a minor effect on overall H trapping. While Cufcc precipitates with a large interface area introduced through intentional Cu alloying might significantly contribute to the H redistribution in a steel microstructure, Cu residuals from the steelmaking process are expected to only have a minor effect on overall H trapping. Acknowledgments The calculations within this work were partly performed at the Vienna Scientific Cluster (VSC). We acknowledge the CINECA award under the ISCRA initiative for the availability of high-performance computing resources. P.H. would like to acknowledge D. Scheiber and F. Moitzi for their help with the Cu9R interface structure setup. Supplementary Materials The following supporting information can be downloaded from https://www.mdpi.com/article/10.3390/ma17225671/s1—POSCAR S1: Cu-9R_Fe_Interface_H_POSCAR.vasp, POSCAR S2: Cu-bcc-001_Fe_Interface_H_POSCAR.vasp, POSCAR S3: Cu-bcc-011_Fe_Interface_H_POSCAR.vasp, POSCAR S4: Cu-fcc_Fe_Interface_H_POSCAR.vasp. Author Contributions Conceptualization, P.H., V.I.R. and M.M.; methodology, P.H. and V.I.R.; software, P.H.; validation, P.H., V.I.R. and M.M.; formal analysis, P.H., V.I.R. and M.M.; investigation, P.H.; resources, V.I.R.; data curation, P.H.; writing—original draft preparation, P.H. and V.I.R.; writing—review and editing, P.H., V.I.R. and M.M.; visualization, P.H.; supervision, V.I.R. and M.M.; project administration, V.I.R.; funding acquisition, V.I.R. All authors have read and agreed to the published version of the manuscript. Institutional Review Board Statement Not applicable. Informed Consent Statement Not applicable. Data Availability Statement POSCAR files of the DFT calculations can be found in the Supplementary Materials. The raw data required to reproduce the computational results findings can be requested from the corresponding author. Conflicts of Interest Authors Philipp Hammer and Vsevolod I. Razumovskiy were employed by the company Materials Center Leoben Forschung GmbH. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest. Funding Statement The authors gratefully acknowledge the financial support under the scope of the COMET program within the K2 Center “Integrated Computational Material, Process and Product Engineering (IC-MPPE)” (project no. 886385). This program was supported by the Austrian Federal Ministries for Climate Action, Environment, Energy, Mobility, Innovation and Technology (BMK) and for Labour and Economy (BMAW), represented by the Austrian Research Promotion Agency (FFG) and the federal states of Styria, Upper Austria, and Tyrol. The financial support of voestalpine Wire Rod Austria GmbH is gratefully acknowledged by the authors. V.I.R. acknowledges the financial support of the Austrian Science Fund (FWF) [I 6756-N]. Footnotes Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. References Associated Data Supplementary Materials Data Availability Statement POSCAR files of the DFT calculations can be found in the Supplementary Materials. The raw data required to reproduce the computational results findings can be requested from the corresponding author.