Journal of the Ceramic Society of Japan (2026), Advance Publication by J-stage DOI https://doi.org/10.2109/jcersj2.26068 JCS - Japan FULL PAPER Cobalt removal capacity on hydroxyapatite-zeolite composite upcycled from blast furnace slag Yoshifumi Kondo1, Tomoyo Goto1,2,³, Yuma Amemiya1,2,3, Yasutaka Kuwahara3,4,‡, Hiromi Yamashita1,3 and Tohru Sekino1,5 1 SANKEN, The University of Osaka, 8–1 Mihogaoka, Ibaraki, Osaka 567–0047, Japan Division of Materials Science, Graduate School of Science and Technology, Nara Institute of Science and Technology (NAIST), 8916–5 Takayama-cho, Ikoma, Nara 630–0192, Japan 3 Division of Materials and Manufacturing Science, Graduate School of Engineering, The University of Osaka, 2–1 Yamadaoka, Suita, Osaka 565–0871, Japan 4 Innovative Catalysis Science Division, Institute for Open and Transdisciplinary Research Initiatives (OTRI), The University of Osaka, 2–1 Yamadaoka, Suita, Osaka 565–0871, Japan 5 3DPTec Integrated Center, The University of Osaka, 2–1 Yamadaoka, Suita, Osaka 565–0871, Japan 2 Upcycling industrial by-products into water treatment materials is a promising strategy for simultaneously achieving resource circularity and water purification. In this study, a hydroxyapatite-zeolite (HAp-ZE) composite upcycled from blast furnace slag, an abundant industrial by-product, was investigated as a sorbent for toxic cobalt ions (Co2+). HAp-ZE removed Co2+ from the solution within a short contact time of 1 h and achieved a removal efficiency of approximately 100 % at Co2+ concentrations of up to 0.4 mmol/L. The sorption isotherm of HAp-ZE fitted well with the Langmuir model. Furthermore, the maximum Co2+ sorption capacity of HApZE, estimated from the sorption isotherm, was comparable to that of a physical mixture of high-purity zeolite and HAp. Sodium ions (Na+) and calcium ions (Ca2+) were released from HAp-ZE during the Co2+ sorption tests. Elemental analysis revealed that Co was distributed in both the zeolite and HAp phases of HAp-ZE. These results suggest that Co2+ removal occurs through cation-exchange reactions in both the zeolite and HAp phases of HAp-ZE. This study demonstrates that the low-cost HAp-ZE produced from blast furnace slag exhibits a Co2+ removal performance comparable to that of its high-purity counterpart, highlighting its potential as a sustainable and economically attractive water purification material. Keywords: Upcycling, Water purification, Blast furnace slag, Hydroxyapatite, Zeolite, Cobalt removal [Received July 21, 2026; Accepted August 17, 2026; Published online September 18, 2026] 1. Introduction The conservation and recycling of water resources have become critical global challenges owing to rapid industrialization, population growth, and increasing freshwater demand. Ensuring access to clean water requires the development of efficient and economically viable water purification materials capable of removing harmful contaminants from water environments.1,2) Heavy metals are a serious concern among various pollutants because they pose long-term risks to both human health and ecosystems. Therefore, significant efforts have been made to develop high-performance sorbents with low production costs.3–5) In particular, cobalt is not only a toxic metal that poses risks to human health and the environment but also a ³ Corresponding author: T. Goto; E-mail: goto@sanken. osaka-u.ac.jp, t.goto@naist.ac.jp ‡ Corresponding author: Y. Kuwahara; E-mail: kuwahara@ mat.eng.osaka-u.ac.jp critical metal widely used in rechargeable batteries and other advanced technologies.2,6) In addition, radioactive cobalt (60Co) generated in nuclear facilities is of environmental concern. Therefore, efficient removal and recovery technologies for cobalt are highly desirable for environmental remediation and sustainable resource management. Recently, the upcycling utilization of industrial byproducts and waste materials as value-added functional materials has attracted increasing attention from the perspectives of both environmental remediation and resource circularity.6–10) Blast furnace slag, a type of steel slag produced during the ironmaking process, is generated in Japan at approximately 19 million tons in 2024.11) Although blast furnace slag is currently utilized in cement production and road construction, there is a growing demand for the exploration of novel value-added applications owing to limited disposal space and increasingly stringent environmental regulations.12,13) Blast furnace slag contains abundant Ca, Si, and Al species, which can be valuable constituents as solid sorbents.11,12) Kuwahara ©2026 The Ceramic Society of Japan This is an Open Access article distributed under the terms of the Creative Commons Attribution License (https://creativecommons.org/licenses/by-nc/4.0/), which permits use, distribution, and reproduction in any medium for non-commercial purposes, provided the original work is properly cited. JCS-Japan Kondo et al.: Cobalt removal capacity on hydroxyapatite-zeolite composite upcycled from blast furnace slag 2.2 Synthesis of HAp-ZE HAp-ZE was synthesized from blast furnace slag according to the previous reports.13,14) 5.0 g of the ball-milled slag was dissolved in 22 mL of 1.0 mol/L H3PO4 aqueous solution for 2 h. 50 mL of 3.0 mol/L NaOH aqueous solution was added dropwise into the suspension. The mixture was then vigorously stirred for 3 h at 80 °C in a water bath. The mixture was transferred to a Teflon bottle and aged in an electric oven at 90 °C for 2 days. The obtained slurry was then filtered, washed with distilled water, and dried overnight at 110 °C. An overview of water purification using hydroxyapatitezeolite composite materials (HAp-ZE) upcycled from blast furnace slag. Fig. 1. et al. demonstrated that hydroxyapatite (HAp) and zeolite composites (HAp-ZE) can be synthesized from blast furnace slag under mild conditions using phosphoric acid, which is highly reactive with calcium.13,14) HAp and zeolite are well-known as promising water purification materials for toxic metal cations.15,16) Therefore, HAp-ZE produced from blast furnace slag is expected to be a promising and cost-effective water treatment material. Although several studies have reported the metal cation removal properties of slag-derived HAp-zeolite composites, their cobalt ion (Co2+) removal performance has not yet been investigated.18,19) Furthermore, no studies have systematically clarified the removal mechanism of slag-derived HAp-zeolite composites through detailed post-sorption characterization. Herein, we investigated the Co2+ removal performance of a HAp-ZE composite upcycled from blast furnace slag (Fig. 1). The Co2+ sorption capacity of HAp-ZE was quantitatively evaluated and compared with those of reference zeolite and HAp to assess the applicability of the upcycled composite as a Co2+ sorbent. In addition, changes in the concentrations of host metal cations released from HAp-ZE during Co2+ sorption were examined to evaluate the contribution of cation-exchange reactions to Co2+ removal. 2. Materials and methods 2.1 Materials Phosphoric acid (H3PO4) and sodium hydroxide (NaOH) were purchased from Nacalai Tesque, Japan. Cobalt nitrate hexahydrate [Co(NO3)2·6H2O] and nitric acid (HNO3) were purchased from FUJIFILM Wako Pure Chemical Corporation, Japan. The blast furnace slag was consisted of 41.5 wt % CaO, 35.8 wt % SiO2, 15.3 wt % Al2O3, 5.48 wt % MgO, and 1.58 wt % Fe2O3, with the remaining fraction consisting of minor components.13,14) Zeolite (X-type zeolite, zeolite 13X) was obtained from Tosoh Corporation, Japan. Hydroxyapatite (HAp, HAP100) was obtained from Taihei Chemical Industrial Co., Ltd., Japan. All reagents were of analytical grade and used without further purification. 2.3 Characterization Powder X-ray diffraction (XRD) patterns were recorded using a D8 ADVANCE (Bruker AXS GmbH, Germany) with Cu K¡ radiation (­ = 1.5418 ¡) at 40 kV and 40 mA. Nitrogen (N2) adsorption–desorption isotherm data were collected at ¹196 °C using BELSORP-max (MicrotracBEL Corp., Osaka, Japan). Samples were preheated at 150 °C for 6 h before the measurement. The specific surface area (SBET) was determined using the Brunauer– Emmett–Teller (BET) method.20) Field-emission scanning electron microscopy (FE-SEM) images were obtained using an SU9000 scanning electron microscope (Hitachi High-Technologies Corporation, Japan) at 20 kV. Elemental analysis of the sorbent was also performed using FE-SEM equipped with energy-dispersive X-ray spectroscopy (EDS, X-MaxN100LE, HORIBA, Ltd., Japan) and X-ray fluorescence (XRF) analysis, using a ZSX-100e wavelength-dispersive X-ray spectroscopy (Rigaku Corporation, Japan). The solution pH after the sorption test was measured using a pH meter (D-52, HORIBA, Ltd., Japan). 2.4 Cobalt sorption test The Co2+ aqueous solution from 0.2 to 4.0 mmol/L was prepared using Co(NO3)2·6H2O without pH adjustment (pH = 5.6–5.8). HAp-ZE and references (Zeolite and HAp) were used as sorbents in the sorption tests. Sorbents (30.0 mg) were placed in plastic tubes, and 20 mL of Co(NO3)2 aqueous solution at various concentrations was added to the tubes. The tubes were shaken at a constant speed of 150 rpm in a mechanical shaker (Bio Shaker, BR43FL, TAITEC Corporation, Japan) at 25 °C for 1 day. Subsequently, the sorbent and solution were separated by filtration, and the sorbents were freeze-dried to obtain powdered samples. The concentrations of Co, Na, and Ca in the solution after sorption testing were analyzed using inductively coupled plasma optical emission spectrometry (ICP-OES; Optima 8300, PerkinElmer Japan Corporation, Ltd., Japan). The sorption results for Co were fitted using the Langmuir equation:21) Ceq Ceq 1 ¼ þ Qmax K Qmax Q ð1Þ where Q is the amount of sorbed Co per gram (mmol/g), Ceq is the equilibrium concentration of Co (mol/L), Qmax is JCS-Japan Journal of the Ceramic Society of Japan (2026), Advance Publication by J-stage the maximum amount of sorbed Co (mmol/g), and K is a constant related to the sorption rate coefficient. The removal efficiency (%) of Co from the test water was calculated using the following equation: Ci  Ceq  100 Ci ð2Þ where Ci and Ceq are the initial concentration of Co (mol/L) and equilibrium concentration of Co in the test solution (mol/L), respectively. The contribution of ion-exchange was calculated using the following equation: 0:5  CNa þ CCa  100 Ci  Ceq ð3Þ where CNa and CCa are the concentrations of Na and Ca in the test solution (mol/L), respectively. 3. Results and discussion 3.1 Characterization of HAp-ZE Figure 2(a) shows powder XRD patterns of HAp-ZE and reference samples (Zeolite and HAp). HAp-ZE corresponded to the mixed crystal phases of FAU-zeolite, P1zeolite, and HAp.14,15,18) Kuwahara et al. previously reported that the metastable phase of FAU-zeolite transformed into the more stable phase of P1-Zeolite with prolonged aging time in HAp-ZE synthesis.13,14) Based on XRF analysis, HAp-ZE consisted of 32.25 wt % zeolite phase, calculated from the chemical composition of (Na2O + SiO2 + Al2O3). In addition, the zeolite phase of HAp-ZE was identified as an X-type zeolite with a molar ratio of SiO2/Al2O3 = 2.85 because FAU-zeolites are referred to as (a) XRD patterns and (b) N2 adsorption–desorption isotherms of HAp-ZE, Zeolite, and HAp. Fig. 2. X- and Y-type according to the molar ratio of 2.0 < SiO2/ Al2O3 < 3.5 and 3.5 < SiO2/Al2O3 < 6.0, respectively. As shown in Fig. 2(b), the N2 adsorption–desorption isotherm of HAp-ZE showed a rapid increase in the amount of absorbed N2 in the range of p/p0 < 0.01, corresponding to the micropores of its zeolite phase. The isotherm of HAp-ZE showed a gradual increase in the range of p/p0 > 0.8, suggesting the aggregation of HAp particles. The isotherm of Zeolite exhibited a type-I isotherm, indicating that Zeolite possesses a micropore structure.23) The type-V isotherm of HAp indicates that it is a nonporous material.23) The specific surface area (SBET) was calculated using the BET method and N2 adsorption isotherm data. The SBET values of the HAp-ZE and reference samples are summarized in Table 1. The SBET of HAp-ZE was around one-quarter of that of Zeolite but 3.5-fold larger than that of HAp because of the small proportion of zeolite phase in HAp-ZE. FE-SEM observations of HAp-ZE revealed two types of crystals with different shapes and sizes [Figs. 3(a) and 3(b)]. One was octahedral microparticles (daverage = 3.96 « 0.59 ¯m), and the other was columnar nanoparticles (daverage = 41.3 « 6.4 nm). EDS mappings of HAp-ZE revealed that the octahedral microparticles were mainly composed of O, Na, Al, and Si, while the columnar Table 1. N2 physisorption data for HAp-ZE and reference samples Sample SBET (m2/g) HAp-ZE Zeolite HAp 171 759 49.3 Fig. 3. (a) FE-SEM image, (b) enlarged image of nanoparticles, and (c) EDS mappings of HAp-ZE. FE-SEM images of (d) Zeolite and (e) HAp. JCS-Japan Kondo et al.: Cobalt removal capacity on hydroxyapatite-zeolite composite upcycled from blast furnace slag nanoparticles consisted of O, Mg, Ca, and P [Fig. 3(c)]. These results suggest that the octahedral particles are zeolite crystals and the columnar particles are HAp crystals. Most of HAp nanoparticles were agglomerated and dispersed on the zeolite crystals. This corresponds well with the N2 adsorption–desorption measurements. Figures 3(d) and 3(e) show the FE-SEM images of the reference samples (Zeolite and HAp). Zeolite and HAp consisted of angular particles with an average particle size of 1.94 « 0.52 ¯m and columnar particles with an average particle size of 70.5 « 13.6 nm. 3.2 Cobalt sorption behavior of HAp-ZE The heavy metal removal capacity of HAp-ZE was evaluated using Co2+ as a probe. Figure 4(a) shows the time dependence of Co2+ removal from HAp-ZE using 1.0 mmol/L Co(NO3)2 aqueous solution. Co2+ was fast removed within the first hour and reached a plateau, with the removal remaining almost constant for up to 24 h. This result suggests that HAp-ZE possesses an affinity for Co2+ and enables its rapid removal from the solution. The Co2+ sorption tests were conducted by shaking the samples at 25 °C for 24 h in a 0.2–4.0 mmol/L Co(NO3)2 aqueous solution. Figure 4(b) presents the removal efficiencies of Co2+ on HAp-ZE and the reference samples. HAp-ZE showed approximately 100 % removal at Co2+ concentrations up to 0.4 mmol/L when 30.0 mg of adsorbent and 20 mL of Co(NO3)2 aqueous solution were used. Figure 4(c) shows the Co2+ sorption isotherms of HAp-ZE and reference samples. The isotherms of all samples were (a) Time course of Co removal using HAp-ZE in a 1.0 mmol/L Co2+ aqueous solution. (b) Removal efficiency, (c) Co2+ sorption isotherms, and (d) Qmax of HAp-ZE, Zeolite, HAp, and a physical mixture of Zeolite and HAp. Condition: Sorbent 30.0 mg, Co2+ aqueous solution 20 mL, 25 at Temperature 25 °C, Time 24 h. well-fitted to the Langmuir model. The maximum sorption density per gram of the sorbents (Qmax) of Co2+ was calculated using Langmuir fitting. As shown in Fig. 4(c), the Omax of Co2+ followed the order Zeolite > HAp-ZE > HAp. The Qmax value for the physical mixture was calculated from the respective activities of Zeolite and HAp. Notably, HAp-ZE possessed a Co2+ removal efficiency comparable to that of the physical mixing of zeolite and HAp [Fig. 4(d)]. These results demonstrate that HAp-ZE synthesized from blast furnace slag, an industrial byproduct, exhibits a Co2+ removal performance comparable to that of the high-purity counterpart. HAp and zeolite are widely known as inorganic ionexchangers capable of removing cations through ionexchange reactions between the host metal ions of the sorbents. Na-type zeolite ion-exchanges between host sodium ions (Na+) in zeolite and external metal cations in a solution. Calcium ions (Ca2+) in HAp exchange with divalent metal cations in the solution. Figures 5(a) and 5(b) show the concentrations of Na+ and Ca2+ released from the sorbents after the Co2+ sorption tests. The amount of Na+ released from the Zeolite exceeded the amount of Co2+ sorbed, whereas the amount of Ca2+ released from the HAp phase was approximately equal to the amount of Co2+ sorbed. Figure 5(c) shows the amounts of Na+ and Ca2+ released from HAp-ZE during the tests, expressed as milliequivalents (meq) to account for differences in ionic charge. For HAp-ZE, the Ca2+ release increased with increasing initial Co2+ concentration. These results suggest an increased contribution of the HAp phase to Co2+ removal at higher Co2+ concentration. Figure 5(d) shows the pH values of the solutions before and after the Co2+ removal tests. The initial pH values Fig. 4. Fig. 5. Concentrations of (a) Na and (b) Ca in the solutions after Co2+ sorption tests. (c) Ratio of released ions from HAp-ZE after Co2+ sorption tests. (d) pH values in the solutions before and after Co2+ sorption tests. Journal of the Ceramic Society of Japan (2026), Advance Publication by J-stage were approximately 5.6–5.8. The solution pH increased after Co2+ sorption for all the samples. The pH values of HAp-ZE and Zeolite were higher than that of HAp, regardless of the Co2+ concentration. The pH values of HAp remained unchanged regardless of the initial concentration, whereas those of Zeolite and HAp-ZE were higher at low initial concentrations. Previous reports have demonstrated that the ion-exchange reactions of Na-type zeolites occur with protons (H+) and Co2+ in the solution.24) In X-type zeolites, Na+ resides in cavities that provide sufficient space to accommodate cations. Therefore, the larger pH increase may be attributed to H+ exchange between Na+ in the zeolite phase and H+ in the solution, in addition to ionexchange with Na+ and Co2+.22,24) In contrast, Co2+ removal by HAp primarily proceeds through ion-exchange with Ca2+ in HAp.25) The Ca2+ sites in HAp preferentially exchange with divalent metal ions, and H+ uptake is expected to be much less favorable than in zeolites, resulting in only a slight increase in the solution pH. This interpretation is consistent with the nearly equivalent amounts of Ca2+ released and Co2+ sorbed [Fig. 5(b)]. Figure 6 shows the XRD pattens of samples after the Co2+ sorption test. There was no significant change in the crystal phases after the Co2+ sorption test compared with those before the test. Furthermore, no diffraction peaks XRD patterns of HAp-ZE, Zeolite, and HAp after the sorption test using 4.0 mmol/L Co2+ aqueous solution. Fig. 6. JCS-Japan corresponding to cobalt-containing compounds were detected in the XRD patterns of all samples after the Co2+ sorption test. Figure 7(a) shows the FE-SEM images and EDS mappings of HAp-ZE after the Co2+ sorption test. No precipitates were observed in HAp-ZE after the Co2+ sorption tests. The elemental mapping of Co was homogeneously distributed in the HAp-ZE sample. These results indicate that Co2+ was sorbed by both the zeolite and HAp phases of HAp-ZE, primarily through ion exchange reactions. Similar to HAp-ZE, no precipitate was observed in the HAp samples [Fig. 7(b)]. The elemental mapping of Co was uniformly distributed in the HAp sample. Furthermore, the pH after the Co2+ sorption test remained nearly constant regardless of the initial Co2+ concentration [Fig. 5(d)], and the amount of released Ca2+ correlated well with the amount of sorbed Co2+ [Figs. 4(c) and 5(b)]. Together with the absence of cobalt-containing phases in the XRD patterns and precipitates in the FE-SEM images after the Co2+ sorption test, these results suggest that Co2+ removal by HAp was predominantly governed by cation-exchange under the present experimental conditions.25,26) In contrast, Fig. 7(c) shows that sheet-like precipitates were observed on the surface of the Zeolite. The elemental mapping of Co overlapped with Zeolite particles and precipitates. In particular, the precipitates consisted of Co and O elements. These results suggest that Co2+ is removed by both ionexchange and precipitation reactions on Zeolite. In Na+exchanged materials, including zeolites, the formation of cobalt hydroxide precipitates has been reported under conditions of high pH and elevated Co2+ concentrations.6,24,27) As shown in Fig. 5(d), the solution pH of the zeolite system decreased markedly at Co2+ concentrations above 2.0 mmol/L, compared with that at lower concentrations. This decrease is likely attributable to the consumption of OH¹ associated with the formation of cobalt hydroxide precipitate. Under such conditions, the precipitates cover the zeolite surface and block the ion-exchange sites, resulting in a decline in Co2+ removal performance.17,24,27) In contrast, no precipitate formation was observed for HAp-ZE, allowing the ion-exchange sites to Fig. 7. FE-SEM image and EDS mappings of (a) HAp-ZE, (b) HAp, and (c) Zeolite after the sorption test using 4.0 mmol/L Co2+ aqueous solution. JCS-Japan Kondo et al.: Cobalt removal capacity on hydroxyapatite-zeolite composite upcycled from blast furnace slag remain accessible even at high Co2+ concentrations. These results demonstrate that HAp-ZE is a promising upcycled sorbent for Co2+ removal from aqueous solutions. 4. Conclusions In this work, we investigated the Co2+ sorption capacity of HAp-ZE converted from blast furnace slag using batch tests with 0.2–4.0 mmol/L Co(NO3)2 aqueous solution. HAp-ZE removed nearly all of the Co2+ from the test solution within the range of initial Co2+ concentrations up to 0.4 mmol/L. The sorption isotherm for HAp-ZE was well-fitted to the Langmuir model, and the calculated maximum sorption capacity (Qmax) was 0.69 mmol/g. The Co2+ removal performance was in the order of Zeolite > HAp-ZE > HAp. Notably, HAp-ZE exhibited a Co2+ sorption capacity equivalent to that of a physical mixture of high-purity Zeolite and HAp. During the Co2+ sorption tests, HAp-ZE released Na and Ca into solutions. Furthermore, FE-SEM and EDS analyses of HAp-ZE after the tests revealed that no detectable precipitates were observed and that Co was uniformly distributed throughout the particles. These results indicate that Co2+ removal by HApZE mainly occurs via an ion-exchange mechanism involving Na+ from the zeolite phase and Ca2+ from the HAp phase. This study demonstrates that an upcycled HAp-ZE composite exhibits Co2+ sorption performance comparable to that of high-purity reference materials and clarifies its ion-exchange-based removal mechanism through systematic post-sorption characterization. These findings highlight the potential of slag-derived HAp-ZE as a costeffective and sustainable sorbent for toxic metal ion removal. Acknowledgments This work was partially supported by the Foundation of Kinoshita Memorial Enterprise and JSPS KAKENHI Grant Number JP25K17915. This work was also supported by the “Dynamic Alliance for Open Innovation Bridging Human, Environment and Materials” and the Cooperative Research Program of “Network Joint Research Center for Materials and Devices” Grant Numbers 20261324 and 20263025 (MEXT, Japan). Y. Kuwahara acknowledges financial support from the Steel Foundation for Environmental Protection Technology and the ISIJ Research Promotion Grant (Tekkou Kenkyu Shinko Josei) from the Iron and Steel Institute of Japan. ICP-OES elemental analysis was performed at the Center for Scientific Instrument Renovation and Manufacturing Support, The University of Osaka, Japan. The authors are grateful to Mr. S. Tamiya (The University of Osaka, Japan) for his technical support in the ICP-OES analysis. XRF analysis was performed at the Comprehensive Analysis Center, SANKEN, The University of Osaka, Japan. References 1) Y. Kondo, T. Goto and T. Sekino, RSC Adv. 11, 18676 (2021). 2) T. Goto, Y. Kondo, S. H. Cho, S. Seino and T. Sekino, Chem. Eng. J. Adv. 12, 100388 (2022). 3) G. Zhao, X. Huang, Z. Tang and X. Wang, Polym. Chem.-UK 9, 3562 (2018). 4) S. Babel and T. A. Kurniawan, J. Hazard. Mater. 97, 219 (2003). 5) K. Sasaki and T. Goto, Ceram. Int. 40, 11649 (2014). 6) Y. Kondo, T. Goto and T. Sekino, RSC Adv. 10, 41032 (2020). 7) J. Jiang, Y. Cao, G. Li, L. Geng, X. Zhang, J. Zhao and C. Liu, ChemPlusChem 90, e20240519 (2025). 8) Y. Kuwahara, A. Hanaki and H. Yamashita, ACS Sustain. Chem. Eng. 10, 372 (2022). 9) Y. Kuwahara and H. Yamashita, ISIJ Int. 57, 1657 (2017). 10) Y. Kuwahara, S. Tamagawa, T. Fujitani and H. Yamashita, B. Chem. Soc. Jpn. 89, 472 (2016). 11) The Japan Iron and Steel Federation, Nippon Slag Association, The Annual report of statistics of Iron and Steel slag (2024); see the website, http://www.slg.jp. 12) Y. Kuwahara, A. Hanaki and H. Yamashita, Green Chem. 22, 3759 (2020). 13) Y. Kuwahara, S. Tamagawa, T. Fujitani and H. Yamashita, J. Mater. Chem. A 1, 7199 (2013). 14) Y. Kuwahara, T. Ohmichi, T. Kamegawa, K. Mori and H. Yamashita, Chem. Lett. 38, 626 (2009). 15) Y. Kuwahara, T. Ohmichi, T. Kamegawa, K. Mori and H. Yamashita, J. Mater. Chem. 19, 7263 (2009). 16) T. Goto and K. Sasaki, Powder Technol. 292, 314 (2016). 17) A. N. V. Azar, A. Duval, F. Langenhorst and L. Wondraczek, J. Am. Ceram. Soc. 107, 6607 (2024). 18) C. Li, X. Li, Y. Yu, Q. Zhang, L. Li, H. Zhong and S. Wang, J. Ind. Eng. Chem. 105, 63 (2022). 19) G. U. Ryu, H. R. Khalid, N. Lee, Z. Wang and H. K. Lee, Minerals-Basel 11, 21 (2020). 20) S. Brunauer, P. H. Emmett and E. Teller, J. Am. Chem. Soc. 60, 309 (1938). 21) I. Langmuir, J. Am. Chem. Soc. 40, 1361 (1918). 22) H. Aono, Y. Matsumoto and Y. Itagaki, J. Ceram. Soc. Jpn. 131, 823 (2023). 23) M. Thommes, K. Kaneko, A. V. Neimark, J. P. Olivier, F. Rodriguez-Reinoso, J. Rouquerol and K. S. W. Sing, Pure Appl. Chem. 87, 1051 (2015). 24) E. Díez, R. Miranda, J. M. López, A. Jiménez, N. Conte and A. Rodrígu, Separations 11, 232 (2024). 25) I. Smičiklas, S. Dimović, I. Plećaš and M. Mitrić, Water Res. 40, 2267 (2006). 26) Z. Zhao, K. Lu, G. ji, H. Zhang, J. Cui, C. Bai, X. Zhao, F. Wang, M. Xia and Y. Zhang, J. Mol. Liq. 386, 122555 (2023). 27) Y. Seo, T. Goto, Y. Amemiya, D. H. Han, Y. Kondo and T. Sekino, J. Eur. Ceram. Soc. 46, 118395 (2026).