HFO-73169 Revision 0 HIGH WASTE LOADING GLASS FORMULATION DEVELOPMENT FOR HIGH-MN HLW, VSL-17R4120-1, REV. 1 Prepared for the U.S. Department of Energy Assistant Secretary for Environmental Management P.O. Box 550 Richland, Washington 99352 HFO-73169 Revision 0 HIGH WASTE LOADING GLASS FORMULATION DEVELOPMENT FOR HIGH-MN HLW, VSL-17R4120-1, REV. 1 K. S. Matlack I. Joseph Vitreous State Laboratory of The Catholic University of America EnergySolutions H. Gan I. L. Pegg Vitreous State Laboratory of The Catholic University of America Vitreous State Laboratory of The Catholic University of America W. K. Kot Vitreous State Laboratory of The Catholic University of America Date Published December 2017 Prepared for the U.S. Department of Energy Assistant Secretary for Environmental Management P.O. Box 550 Richland, Washington 99352 By Lynn M Ayers at 10:31 am, Feb 26, 2026 Release Approval Date HFO-73169 Revision 0 TRADEMARK DISCLAIMER Reference herein to any specific commercial product, process, or service by tradename, trademark, manufacturer, or otherwise, does not necessarily constitute or imply its endorsement, recommendation, or favoring by the United States Government or any agency thereof or its contractors or subcontractors. This report has been reproduced from the best available copy. Printed in the United States of America VSL-17R4120-1 Final Report High Waste Loading Glass Formulation Development for High-Mn HLW prepared by Keith S. Matlack, Hao Gan, Wing K. Kot, and Ian L. Pegg Vitreous State Laboratory The Catholic University of America Washington, DC 20064 and Innocent Joseph Atkins Energy Federal EPC, Inc. Calverton, MD 20705 for Department of Energy Office of River Protection July 10, 2017 Rev. 1, 12/5/17 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 TABLE OF CONTENTS LIST OF TABLES ...................................................................................................................................... 5 LIST OF FIGURES .................................................................................................................................... 7 LIST OF ABBREVIATIONS .................................................................................................................... 9 SECTION 1.0 INTRODUCTION............................................................................................................ 10 1.1 TEST OBJECTIVES........................................................................................................................... 12 1.2 QUALITY ASSURANCE .................................................................................................................... 12 1.3 DM100 MELTER SYSTEM .............................................................................................................. 13 1.3.1 DM100 Feed System ............................................................................................................. 13 1.3.2 Melter System ........................................................................................................................ 13 1.3.3 Off-Gas System ...................................................................................................................... 13 1.4 EXPERIMENTAL METHODS ............................................................................................................. 14 1.4.1 Feed Conversion by Vertical Gradient Furnace (VGF) Testing ........................................... 14 1.4.2 Feed Composition and General Properties .......................................................................... 14 1.4.3 Crucible and Melter Product Glasses ................................................................................... 15 1.4.3.1 Viscosity .............................................................................................................................. 15 1.4.3.2 Electrical Conductivity........................................................................................................ 15 1.4.3.3 Product Consistency Test (PCT) ......................................................................................... 16 1.4.3.4 Toxicity Characteristic Leaching Procedure (TCLP) ......................................................... 16 1.4.3.5 Secondary Phases................................................................................................................ 16 1.4.3.6 Crystalline Phases by X-Ray Diffraction ............................................................................ 17 1.4.3.7 Mössbauer Spectroscopy .................................................................................................... 17 SECTION 2.0 WASTE SIMULANT, GLASS FORMULATION, AND MELTER FEED ANALYSIS ................................................................................................................................................ 18 2.1 HIGH MANGANESE SIMULANT COMPOSITION ............................................................................... 18 2.2 MANGANESE FORMS IN HANFORD HLW AND MELTER FEED ....................................................... 19 2.3 DEVELOPMENT OF GLASS FORMULATION FOR HIGH MN HLW .................................................... 20 2.3.1 High Manganese HLW and Glass Formulation Strategy ..................................................... 20 2.3.2 Formulation of High-Mn HLW Glasses at 45 wt% Waste Loading ...................................... 20 2.3.3 Formulation of High-Mn HLW Glasses at 40 wt% Waste Loading ...................................... 21 2.3.4 Formulation of High-Mn HLW Glasses at 35 wt% Waste Loading ...................................... 21 2.3.5 Formulation of High-Mn HLW Glasses at 32 wt% Waste Loading ...................................... 22 2.3.6 Formulation at 35 wt% Waste Loading to Reduce PCT Releases ........................................ 22 2.3.7 Selection of HLW-HMn-20 Glass Formulation for Melter Testing....................................... 22 2.4 ANALYSIS OF MELTER FEED SAMPLES .......................................................................................... 23 2.4.1 General Properties ................................................................................................................ 23 2.4.2 Chemical Composition .......................................................................................................... 24 2.4.4 Vertical Gradient Furnace .................................................................................................... 24 SECTION 3.0 DM100 MELTER OPERATIONS ................................................................................. 26 3 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 SECTION 4.0 GLASS PRODUCT ANALYSIS..................................................................................... 30 4.1 COMPOSITIONAL ANALYSIS OF DISCHARGE AND DIP GLASS SAMPLES ........................................ 30 4.2 CHEMICAL DURABILITY OF DISCHARGE GLASSES ........................................................................ 31 4.3 SEM AND MÖSSBAUER ANALYSIS OF MELTER GLASS SAMPLES ................................................. 32 SECTION 5.0 MONITORED OFF-GAS EMISSIONS ........................................................................ 33 5.1 PARTICULATE SAMPLING ............................................................................................................... 33 5.2 PARTICULATE SAMPLED FROM OFF-GAS SYSTEM ........................................................................ 34 5.3 GASES MONITORED BY FTIR ......................................................................................................... 35 SECTION 6.0 SUMMARY AND CONCLUSIONS .............................................................................. 36 SECTION 7.0 REFERENCES ................................................................................................................. 40 4 List of Tables Page # Table 1.1 Ranking Basis for Feed Conversion after 30 Minute VGF Test. T-1 Table 2.1 Calcined Composition (wt%) of High-Manganese HLW Simulant. T-2 Table 2.2 Composition of High-Manganese HLW Simulant to Produce 100 kg of Waste T-3 Oxide (21.50 wt% total solids). Table 2.3 Target and XRF Analyzed Compositions of HLW-HMn Glasses. T-4 Table 2.4 Summary of Characterization Results for HLW-HMn Glasses. T-7 Table 2.5 Viscosity and Electrical Conductivity of Selected HLW-HMn Glass Melts. T-9 Table 2.6 PCT Releases of Selected HLW-HMn Glasses. T-12 Table 2.7 TCLP Results (ppm) of Selected HLW-HMn Glasses. T-13 Table 2.8 Composition (wt%) and Properties of High Manganese (Waste Batch 3939) T-14 HLW Simulant and Glass Formulation HLW-HMn-20 with 35% Waste Loading. Table 2.9 Composition of Melter Feed to Produce 100 kg of Target Glass from High T-15 Manganese (Waste Batch 3939) HLW Simulant (Target Glass Yield = 500 g/l). Table 2.10 Characteristics of Melter Feed Samples with the HLW-HMn-20 Formulation T-16 and Various Forms of Manganese. Table 2.11 XRF and DCP Analyzed Compositions of As-Received Vitrified Melter T-17 Feed Samples (wt%). Table 2.12 XRF and DCP Analyzed Compositions of Vitrified Melter Feed Samples for the T-18 HLW-HMn20 Formulation and Various Forms of Manganese (wt%). Table 2.13 VGF Test Results for HLW-HMn-20 Formulation with Various Forms of T-19 Manganese Compared to Results for a High Iron Formulation with Different Iron Sources. Table 3.1 Summary of Results from DM100 Tests while Processing the HLW-HMn-20 T-20 Glass Composition and Various Manganese Sources. Table 3.2 Steady-State Production Rates Achieved on the DM100 Melter with Various T-22 Hanford HLW Streams at a Glass Temperature of 1150oC and Feed Solids Content of 500 g Glass Per Liter. Table 3.3 Steady-State Production Rates Achieved with Iron and Manganese Limited HLW T-23 Compositions and Different Forms of the Waste Loading Limiting Components. Table 3.4 Summary of Measured DM100 Parameters while Processing the HLW-HMn-20 T-24 Glass Composition and Various Manganese Sources. Table 4.1 List of Glass Discharged and Masses During Tests with the HLW-HMn-20 T-26 Formulation and Various Forms of Manganese. Table 4.2 XRF Analyzed Composition of Glass Discharged During DM100 Testing T-29 with the HLW-HMn-20 Glass Composition and MnO as the Manganese Source (wt%). Table 4.3 XRF Analyzed Composition of Glass Discharged During DM100 Testing with T-32 the HLW-HMn-20 Glass Composition and MnO2 as the Manganese Source (wt%). Table 4.4 XRF Analyzed Composition for Glass Discharged During DM100 Testing T-33 with the HLW-HMn-20 Glass Composition and MnCO3 as the Manganese Source (wt%). Table 4.5 XRF Analyzed Composition of Dip Samples Taken After DM100 Melter T-34 Tests (wt%). Table 4.6 Comparison of XRF Analysis of Terminal Discharged Glass from each Test T-35 and Target Composition. 5 Table 4.7 PCT Results for Melter and Crucible Glasses. T-35 Table 4.8 TCLP Results for Melter and Crucible Glasses (mg/l). T-36 Table 4.9 Volume Percent Crystalline Spinels and Mössbauer Analysis of Melter Glasses. T-37 Table 4.10 Description of Crystalline Phases Identified by SEM. T-37 Table 5.1 Results from DM100 Off-Gas Emission Samples while Processing the T-38 HLW-HMn-20 Glass Composition and Various Manganese Sources. Table 5.2 Analysis of Mineral Content in Material Collected from Cyclones in the T-40 Off-gas System. Table 5.3 XRF and DCP-AES Analysis of Material Collected from Cyclones in the Off-gas T-41 System After Testing (wt%). Table 5.4 Concentrations (ppmv) of Selected Species in DM100 Exhaust Measured by T-42 FTIR Spectroscopy (ppmv). 6 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 List of Figures Page # Figure 1.1 Schematic diagram of DuraMelter 100 vitrification system. F-1 Figure 1.2.a Schematic diagram showing cross-section through the DM100-BL-melter. F-2 Plan view showing locations of lid ports Figure 1.2.b Schematic diagram showing cross-section through the DM100-BL melter. F-3 Figure 1.2.c Schematic diagram showing cross-section through the DM100-BL melter. F-4 Figure 1.3 Schematic drawing of vertical gradient furnace (VGF) for feed conversion test. F-5 Figure 1.4 Temperature gradient (inside the loaded ceramic crucible) of the vertical F-6 gradient furnace (VGF). Figure 2.1 Al2O3 and MnO Concentrations in Hanford HLW. F-7 Figure 2.2 Fe2O3 and MnO Concentrations in Hanford HLW. F-8 Figure 2.3 Na2O and MnO Concentrations in Hanford HLW. F-9 Figure 2.4 SEM images and EDS spectra of glass HLW-HMn-20 after 70 hours at F-10 a) 950C, b) 900C, c) 850C and d) 800C. Figure 2.5 Images of feed sample of XBL-F-19A (MnO as manganese source) F-12 after vertical gradient furnace tests (17 g glass yield). Figure 2.6 Images of feed sample of XBL-F-79A (MnO2 as manganese source) after F-13 vertical gradient furnace tests (17 g glass yield). Figure 2.7 Images of feed sample of XBL-F-96A (MnCO3 as manganese source) after F-14 vertical gradient furnace tests (17 g glass yield). Figure 2.8 Top view and cross section view of VGF samples of feeds for formulation HLW-HMn-10 with different forms of manganese and reductant. F-15 Figure 3.1.a Glass production rates (hourly moving averages and cumulative) for DM100 F-17 tests with the HLW-HMn-20 glass composition; MnO as the manganese source with optimized and nominal bubbling. Figure 3.1.b Glass production rates (hourly moving averages and cumulative) for DM100 F-18 tests with the HLW-HMn-20 glass composition; MnO2 and MnCO3 as the manganese sources. Figure 3.1.c Cumulative glass production rates for DM100 tests with the HLW-Mn20 glass F-19 composition and various manganese sources. Figure 3.1.d Instantaneous glass production rates for DM100 tests with the HLW-Mn20 F-20 glass composition and various manganese sources. Figure 3.1.e Glass production rates for DM100 tests with the manganese and iron-limited F-21 glass compositions and various waste loading limiting component sources. Figure 3.2.a Glass temperatures during DM100 tests with the HLW-HMn-20 glass F-22 composition; MnO as the manganese source with optimized and nominal bubbling. Figure 3.2.b Glass temperatures during DM100 tests with the HLW-HMn-20 glass F-23 composition; MnO2 and MnCO3 as the manganese sources. Figure 3.3.a Plenum temperatures during DM100 tests with the HLW-HMn-20 glass F-24 composition; MnO as the manganese source with optimized and nominal bubbling. Figure 3.3.b Plenum temperatures during DM100 tests with the HLW-HMn-20 glass F-25 composition; MnO2 and MnCO3 as the manganese sources. 7 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Figure 3.4.a Electrode temperatures and power during DM100 tests with the HLW-HMn-20 glass composition; MnO as the manganese source with F-26 optimized and nominal bubbling. Figure 3.4.b Electrode temperatures and power during DM100 tests with the F-27 HLW-HMn-20 glass composition; MnO2 and MnCO3 as the manganese sources. Figure 3.5.a Melt pool resistance and total electrode power during DM100 tests with the F-28 HLW-HMn-20 glass composition; MnO as the manganese source with optimized and nominal bubbling. Figure 3.5.b Melt pool resistance and total electrode power during DM100 tests with the F-29 HLW-HMn-20 glass composition; MnO2 and MnCO3 as the manganese sources. Figure 3.6.a Melt pool bubbling during DM100 tests with the HLW-HMn-20 glass F-30 composition; MnO as the manganese source with optimized and nominal bubbling. Figure 3.6.b Melt pool bubbling during DM100 tests with the HLW-HMn-20 glass F-31 composition; MnO2 and MnCO3 as the manganese sources. Figure 4.1.a DM100 product and target glass compositions determined by XRF. F-32 Figure 4.1.b DM100 product and target glass compositions determined by XRF. F-33 Figure 4.1.c DM100 product and target glass compositions determined by XRF. F-34 Figure 4.1.d DM100 product and target glass compositions determined by XRF. F-35 Figure 4.1.e DM100 product and target glass compositions determined by XRF. F-36 Figure 4.1.f DM100 product and target glass compositions determined by XRF. F-37 Figure 4.1.g DM100 product and target glass compositions determined by XRF. F-38 Figure 4.2 SEM images and EDS spectra of a) XBL-G-58A discharged after F-39 MnO tests b) XBL-G-89C discharged after MnO2 test. Figure 5.1.a FTIR monitored NO emissions while processing the HLW-HMn-20 F-40 glass composition. Figure 5.1.b FTIR monitored CO2 emissions while processing the HLW-HMn-20 F-41 glass composition. Figure 5.1.c FTIR monitored water content of exhaust while processing the F-42 HLW-HMn-20 glass composition. 8 List of Abbreviations ANL-LRM Argonne National Laboratory – Low Activity Reference Material ASME American Society of Mechanical Engineers BBI Best Basis Inventory BNI Bechtel National Incorporated CUA The Catholic University of America DCP-AES Direct Current Plasma Atomic Emission Spectroscopy DM DuraMelter DOE Department of Energy DWPF-EA Defense Waste Processing Facility – Environmental Assessment EDS Energy Dispersive X-Ray Spectroscopy FTIR Fourier Transform Infrared Spectroscopy IC Ion Chromatography HEPA High-Efficiency Particulate Air Filter HLW High Level Waste HTWOS Hanford Tank Waste Operations Simulator LAW Low Activity Waste NIST National Institute of Standards and Technology NQA Nuclear Quality Assurance ORP Office of River Protection PCT Product Consistency Test QAPP Quality Assurance Project Plan QARD Quality Assurance Requirements and Description SEM Scanning Electron Microscopy TCLP Toxicity Characteristic Leach Procedure UTS Universal Treatment Standard VGF Vertical Gradient Furnace VSL Vitreous State Laboratory WTP Hanford Tank Waste Treatment and Immobilization Plant XRD X-Ray Diffraction XRF X-Ray Fluorescence Spectroscopy 9 SECTION 1.0 INTRODUCTION Projections of the number of high level waste (HLW) canisters to be produced in the Hanford Tank Waste Treatment and Immobilization Plant (WTP) (e.g., [1]) are based upon the inventory of the tank wastes, the anticipated performance of the sludge treatment processes, and current understanding of the capability of the borosilicate glass waste form. The WTP HLW melter design, unlike earlier Department of Energy (DOE) melter designs, incorporates a glass bubbler system. The bubblers create active glass pool mixing and thereby improve heat and mass transfer and glass melting rate. The WTP HLW melters each have a glass surface area of 3.75 m 2 and depth of ~1.1 m. The two melters in the HLW facility together are designed to produce up to 7.5 MT of glass per day at 100% availability. Further increases in HLW waste processing rates can potentially be achieved by optimization of the feed and glass formulations, increasing the waste loading in the glass product, and by increasing the melter operating temperature above 1150C. Increasing the waste loading also has the added benefit of decreasing the number of canisters for storage. The baseline WTP glass formulation efforts have been conservative in terms of achievable waste loadings. These baseline formulations have been specified to ensure that the glasses are homogenous, contain essentially no crystalline phases, are processable in joule- heated, ceramic-lined melters, and meet WTP contract requirements. The overall WTP mission will require the immobilization of tank waste compositions that are dominated by mixtures that include aluminum, chromium, bismuth, iron, phosphorous, zirconium, and sulfur compounds as waste loading limiting components. In order to improve waste loadings, DOE’s Office of River Protection (ORP) initiated a testing program to develop and characterize HLW glasses for wastes that are limited by Al, Al plus Na, Bi, and Cr [1, 2]. Results of that work have demonstrated the feasibility of increases in waste loading from about 25 wt% to 33-50 wt% (based on oxide loading) in the glass, depending on the waste stream. It is expected that these higher waste loading glasses will reduce the HLW canister production requirement by about 25% or more [3]. Furthermore, it has been shown that a key technological risk area relates to the strong dependence of glass production rate on waste composition [3]. The extent of this variation across the full spectrum of HLW waste types needs to be quantified in order to accurately project waste treatment rates. Under a separate contract with Bechtel National Incorporated (BNI) to support the WTP, the Vitreous State Laboratory (VSL) of the Catholic University of America (CUA) has developed and tested glass formulations for WTP HLW compositions to provide data to meet the WTP contract requirements and to support system design activities [4-9]. That work was based upon small­scale batch melts (“crucible melts”) using waste simulants. Selected formulations were also tested in continuously fed, joule-heated melters, DuraMelter (DM)100 and DM1200 [10-15]. That testing was directed towards waste streams from the then-planned early feed tanks for the WTP (i.e., AZ-101, AZ-102, C-106/AY-102, and C-104/AY-101). These wastes are high 10 in iron (AZ-101, AZ-102 and C-106/AY-102) or thorium (C-104/AY-101) and are significantly different from those used in subsequent enhancement tests performed for ORP (i.e., wastes limited by Al, Al/Na, Bi, and Cr). Baseline glass formulations to treat these high-Fe wastes were developed under the BNI contract. During that time, the throughput requirement for the HLW melter was initially 400 kg/(m2·day), which was subsequently increased to 800 kg/(m2·day). As a result, the baseline high-Fe HLW glass formulations for WTP perform only slightly better than the 800 kg/(m2·day) processing rate requirement. Furthermore, the baseline waste loadings for the Fe-limited HLW compositions are only slightly higher than the BNI contract minimum. In subsequent work performed for ORP on other HLW compositions, VSL has developed small- scale test methods to assess the processing rates of melter feeds and included them as an integral part of glass formulation development. This methodology was used successfully to develop glass formulations for high-Al Hanford HLW that showed processing rates in excess of 2000 kg/(m2·day) while achieving high waste loadings. The same methodology can be applied to the development of improved glass formulations for other Hanford HLW streams in order to provide ORP with a significantly more robust operating envelope with reduced risk of throughput shortfalls. Consequently, a wide range of HLW Hanford waste streams rich in constituents such as iron [16], bismuth [17], sulfur [18, 19], chromium [20], strontium [21], and zirconium [22], which have the potential to limit waste loadings and production rates, are being addressed in a series of glass formulation development and melter testing tasks. This report describes the results from work performed to develop and test new glass and feed formulations in order to increase waste loadings for Hanford HLW with high concentrations of manganese. A further objective of the work was to determine the effect of the form of manganese in Hanford HLW on feed processing rates. A number of HLW batches to be processed at the WTP have manganese concentrations that extend above about thirteen weight percent on an oxide basis. These high manganese HLW streams frequently contain significant amounts of chromium, iron, and nickel, which together have the tendency to form secondary phases such as spinels that can limit waste loading or lead to poor cold cap behavior and slow processing rates [23]. Previous studies for ORP have explored some of the HLW streams that contain relatively high concentrations of iron and chromium with manganese [23]; however, those studies did not focus on HLW streams for which glass waste loading is manganese limited. Manganese is present in Hanford tank waste in a variety of forms including MnO, MnO2, MnCO3, spinels and hydroxides with iron and nickel, and oxalates [24-26]. These differences in manganese form have the potential to affect waste and melter feed rheology, feed processing rates, and the extent of crystalline phases in the glass product, as has been observed with different forms of aluminum and iron in HLW waste simulants [27-29]. In particular, glass formulation development for high manganese HLW can be challenging due to spinel formation, especially in the presence of other spinel forming elements such as iron, chromium, and nickel [6, 12, 23, 30]. In addition, foaming of the glass pool during vitrification has been attributed to manganese oxidation state changes [13-15] and this may also be affected by the form of manganese in the waste. These issues were addressed by developing glass formulations for a Hanford HLW stream with high concentrations of manganese followed by melter testing with the selected glass composition with feed containing manganese in three different forms likely to be present in Hanford tank wastes. A similar strategy was employed successfully for determining 11 the differences in the feed and glass properties and feed processing characteristics of HLW feeds with different forms of aluminum and iron [27-29]. Testing was conducted to identify glass and melter feed formulations that optimize waste loading and waste processing rate while meeting all processing and product quality requirements. A high-manganese HLW composition derived from the inventory data on insoluble components from the Best Basis Inventory (BBI) Hanford Tank Waste Operations Simulator (HTWOS) model run (April 17, 2011) [31] was used as the basis for the present glass formulation development and melter testing. The work included preparation and characterization of crucible melts to evaluate the effects of waste loading on glass properties and the maximum waste loadings that can be achieved. Testing included assessment of melt rate using a Vertical Gradient Furnace (VGF) system to identify formulations with high melt rates as well as high waste loadings. The results from crucible-scale testing supported subsequent melter tests on a DM100 vitrification system designed to examine the effects of enhanced glass and feed formulations on waste processing rate and product quality. DM100 melter tests were conducted with feeds containing the different forms of manganese under nominal conditions (1150°C glass temperature, 9 lpm bubbling) so that the effect of the form of manganese on feed processing rate and processing characteristics could be determined. Samples of the glass product were collected and analyzed for composition and crystalline phases. Data on processing rate and any processing difficulties such as melt pool foaming, off-gas composition, and system operating parameters were collected. This work builds on previous work performed at the VSL for ORP to increase waste loadings and processing rates of HLW glass formulations [3, 16, 20-22, 32, 33]. The testing was performed according to the Test Plan that was developed for this work [34]. 1.1 Test Objectives One of the primary objectives of the work described herein was to develop and identify HLW glass compositions and glass forming additive blends that achieve high waste loadings and processing rates for high manganese HLW streams while maintaining acceptable glass properties. Another objective was to determine the effect of the form of manganese (MnO, MnO2, MnCO3) on feed processing properties, glass production rates, and product quality while vitrifying a high manganese HLW stream. This was accomplished through a combination of crucible-scale tests, vertical gradient furnace tests, and confirmation tests on a DM100 melter system. 1.2 Quality Assurance This work was conducted under a quality assurance program that is based on Nuclear Quality Assurance (NQA)-1 2008 that is in place at the VSL. The program is compliant with applicable criteria of 10 CFR 830.120; Office of Civilian Waste Management DOE/RW-0333P, Quality Assurance Requirements and Description (QARD) Revision 20; the American Society of Mechanical Engineers (ASME) NQA-1, 2008 including NQA-1a-2009 addenda; and DOE Order 414.1 D, Quality Assurance. This program is supplemented by a Quality Assurance Project Plan (QAPP) for ORP WTP work [35] that is conducted at VSL. Test and procedure requirements by 12 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 which the testing activities are planned and controlled are also defined in that plan. The program is supported by VSL standard operating procedures that were used for this work [36]. 1.3 DM100 Melter System 1.3.1 DM100 Feed System A schematic diagram of the DM100 vitrification system is shown in Figure 1.1. The melter feed is introduced in batches into a feed container that is mounted on a load cell for weight monitoring. The feed is stirred with a variable speed mixer and constantly recirculated except for periodic, momentary interruptions during which the weight is recorded. A peristaltic pump is used to provide a uniform delivery of feed to the melt surface. Feed is directed from the recirculation loop that extends to the top of the melter and then diverted to the peristaltic pump, which regulates the flow of feed through a Teflon-lined feed line and water-cooled feed tube into the melter. 1.3.2 Melter System Cross-sectional diagrams of the DM100-BL melter are shown in Figures 1.2.a-c. The DM100-BL unit is a ceramic refractory-lined melter fitted with five electrodes: two pairs of opposing Inconel 690 plate electrodes and a bottom electrode. Power can be supplied in either three-phase or single-phase configurations. All of the tests in the present work were performed with the upper and lower electrodes on each side connected together and powered by a single-phase supply; the bottom electrode was not powered. Melt pool agitation is achieved by either a removable lance bubbler entering from the top of the melter or a permanent bubbler installed through the bottom electrode. In these tests, the lance bubbler was used. The glass product is removed from the melter by means of an airlift discharge system. The melter has a melt surface area of 0.108 m 2 and a variable glass inventory of between 110 kg, when only the P P bottom pair of electrodes is used, and about 170 kg when both pairs of electrodes are used, which was the case in the present tests. 1.3.3 Off-Gas System For operational simplicity, the DM100-BL is equipped with a dry off-gas treatment system involving gas filtration operations only. Exhaust gases leave the melter plenum through a film cooler device that minimizes the formation of solid deposits. The film-cooler air has constant flow rate and its temperature is thermostatically controlled. Consequently, under steady-state operating conditions, the exhaust gases passing through the transition line (between the melter and the first filtration device) can be sampled at constant temperature and airflow rate. The geometry of the transition line conforms to the requirements of the 40-CFR-60 air sampling techniques. Immediately downstream of the transition line are cyclonic filters followed by conventional pre-filters and high efficiency particulate air (HEPA) filters. The temperature of the cyclonic filters is maintained above 150°C while the temperatures in the HEPAs are kept 13 sufficiently high to prevent moisture condensation. The entire train of gas filtration operations is duplicated and each train is used alternately. An induced draft fan completes the system. 1.4 Experimental Methods 1.4.1 Feed Conversion by Vertical Gradient Furnace (VGF) Testing Figure 1.3 shows a schematic diagram of the VGF setup. The temperature gradient inside the VGF is maintained by two separate sets of heating elements, both of which are arranged in cylindrical form and aligned along their axes. The inner heater is set at 1150oC, which is the nominal temperature of the glass pool, and the ambient heater is set at 600oC, which is similar to the melter plenum temperature. A ceramic crucible (4 inches tall) is used to contain the reacting melter feed. The temperature gradient in the test crucible is shown in Figure 1.4. For a typical feed conversion test, 10 grams of glass of identical chemical composition to the test feed (expressed on an oxide basis) is preheated in the ceramic crucible positioned in the inner heater before the dried melter feed (to yield 17 grams of glass) is introduced. Feed reactions under the controlled temperature gradient are allowed to continue for the designated test duration (typically, from 30 to 90 minutes) and then stopped by rapid cooling in room temperature air. The top surface of the reacted feed material is then inspected and photographed. The crucibles with their feed contents are then cross-sectioned to reveal the conversion progress of feed blends. The saw cuts of the crucibles are performed dry (without lubricant) to avoid loss of any soluble material. To characterize the reacted feed material, visual inspection and digital imaging of the top (by photography) and cross section (using an optical scanner) of the reacted sample are performed. The VGF results are used to evaluate the melt rate on a relative scale using the degree of melting that has occurred, the structure of the feed materials that are undergoing reaction and transformation, and the feed conversion progression with time. A VGF sample showing relatively more feed conversion and melting is classified as fast whereas a sample showing relatively less feed conversion and melting is classified as slow. In cases where multiple VGF samples are tested, a numerical ranking of relative melt rate is assigned based on a correlation using feeds that were tested on the VGF and whose melt rates had been determined previously in DM100 melter tests [27]. The numerical rankings of feed samples based on the extent of feed conversion from observation of the top and cross section of VGF samples is given in Table 1.1. The rankings span the range of 1 to 6, with a feed sample ranked 1 expected to exhibit a fast processing rate and a feed sample ranked 6 expected to show a slow processing rate. 1.4.2 Feed Composition and General Properties Feed samples were taken directly from as-received drums and the melter feed recirculation line during each test. Feed samples were poured into a platinum/gold crucible and placed into a programmed furnace for drying and fusion to form a glass. The glass produced from this fusion was ground to less than 200 mesh and sealed in 20-ml vials for subsequent analysis by X-ray fluorescence spectroscopy (XRF), or by acid digestion followed by 14 direct-current plasma atomic emission spectroscopy (DCP-AES) on the resulting solution. The feed samples were also characterized for their density, pH, water content, and glass yield. 1.4.3 Crucible and Melter Product Glasses The glass product is discharged from the melter into 5-gallon steel pails periodically using an air-lift system. The discharged product glass is sampled at the end of each test by removing sufficient glass from the top of the pails for compositional analysis and secondary phase determination. In addition, sufficient glass from the end of tests with each form of manganese was collected to perform the Product Consistency Test (PCT, 7 days at 90 oC) and Toxicity Characteristic Leaching Procedure (TCLP). Prior to those tests, characterization with respect to PCT, TCLP, melt electrical conductivity, melt viscosity, and secondary phases was performed on the crucible melt compositions to select a formulation for melter testing that is compliant with the present WTP contract requirements. All of these procedures are routinely conducted at VSL and, therefore, standard operating procedures are in place [36]. Sample preparation for chemical analysis begins with size reduction and sieving. All samples are then subjected to XRF analysis to determine the concentrations of all elements except boron and lithium. A series of National Institute of Standards and Technology (NIST) reference materials are used for confirmation of the XRF data. Boron and lithium are determined by total acid dissolution of ground glass samples in HF/HNO3 and subjecting the resulting solutions to DCP-AES analysis. Glass samples from melter tests with different manganese sources were also analyzed for iron redox state by Mössbauer Spectroscopy using glass prepared as for the XRF analysis. 1.4.3.1 Viscosity The melt viscosity, η, is measured using a Brookfield viscometer. Measurements are performed in the temperature range of 950-1250ºC and the data are interpolated to standard temperatures using the Vogel-Fulcher equation: ln η = [A/(T-To)]+B, where A, B, and To are fitting parameters. The equipment is calibrated at room temperature using standard oils of known viscosity and then checked at 950-1250ºC using a NIST standard reference glass (SRM 711). Both precision and accuracy of the viscosity measurements are estimated to be within ±15 relative%. 1.4.3.2 Electrical Conductivity The electrical conductivity, σ, of each glass is determined by measuring the resistance of the glass melt as a function of frequency using a calibrated platinum/rhodium electrode probe attached to a Agilent model 4194A impedance analyzer. Measurements are performed over similar temperature ranges to those employed for the melt viscosity measurements. The results are analyzed to obtain the DC electrical conductivity. The electrical conductivity data are then interpolated to standard temperatures using the Vogel-Fulcher equation: ln  = [A/(TTo)] + B, 15 where A, B and To are fitting parameters. Estimated uncertainties in the electrical conductivity measurements are  20 relative%. 1.4.3.3 Product Consistency Test (PCT) The product consistency test (PCT; ASTM C 1285) [37] is used to evaluate the relative chemical durability of glasses by measuring the concentrations of the chemical species released from 100-200 mesh crushed glass (75-149 μm) to the test solution (de-ionized water in this case). PCTs on the HLW glasses are performed at 90ºC, in accordance with the current WTP contract requirement. The ratio of the glass surface area to the solution volume for this test is about 2000 m-1 (typically, 4 g of 100-200 mesh glass is immersed in 40 ml of deionized water). All tests are conducted in triplicate, in 304L stainless steel vessels, and in parallel with a standard glass included in each test set. The internal standard is the Argonne National Laboratory – Low Activity Reference Material (ANL-LRM) glass [38] and/or the Defense Waste Processing Facility – Environmental Assessment (DWPF-EA) glass [39], both of which have undergone round-robin testing. The leachates are sampled at predetermined times, the first of which is seven days. One milliliter of sampled leachate is mixed with 20 ml of 1M HNO3 and the resulting solution is analyzed by DCP-AES; another 3 ml of sampled leachate is used for pH measurement. 1.4.3.4 Toxicity Characteristic Leaching Procedure (TCLP) The TCLP was performed at VSL using SW-846 Method 1311, which employs leaching of crushed glass (< 3/8”) in a sodium acetate buffer solution for 18 hours at 22C with constant end-over-end agitation. A mass of about 100 grams of glass is leached in 2 liters of TCLP extract, according to the extraction method for non-volatiles. The surface area to volume ratio for this test is about 20 m-1, which is about two orders of magnitude lower than that in the PCT. The leachates are analyzed by DCP-AES according to VSL standard operating procedures. 1.4.3.5 Secondary Phases Secondary phases in the glass samples were determined by optical microscopy and scanning electron microscopy coupled with energy dispersive X-ray spectroscopy (SEM-EDS) in combination with X-ray diffraction (XRD) analysis. Secondary phases due to crystallization and phase separation can be identified using these methods. The samples for SEM analysis are processed by grinding and sieving (-18 mesh, < 1 mm) in order to provide a representative measure of the overall crystal fraction in the sample. Ground glass samples are mounted in epoxy, polished to expose cross sections of the glass grains, coated with carbon, and examined using SEM/EDS. The amount of crystals in glass samples was determined by SEM in conjunction with image analysis. 16 1.4.3.6 Crystalline Phases by X-Ray Diffraction Quantitative XRD was used to determine the crystal content in glasses and in solids from the cyclone filter in the off-gas system. Powder diffraction data were gathered using a Thermo- Fisher X-tra theta-theta diffractometer fitted with a Cu X-ray tube. Glass samples were ground and sieved to 325 mesh. Five weight percent of a corundum internal standard was mixed with the powdered sample for quantitative analysis of the crystalline phases. Each powder pattern was scanned from 5 to 80 degrees 2 theta using a collection time of 2 seconds per data point. JADE9 software was used to perform the search-match identification of the crystalline phases as well as the whole pattern fitting to determine the weight percent of each crystalline phase in the sample. 1.4.3.7 Mössbauer Spectroscopy Mössbauer spectroscopy is an analytical technique that utilizes the recoil-free emission and resonant absorption of gamma rays by nuclei bound in solids. The energies of the gamma ray emitter (source) and absorber (sample) have to be closely matched and, therefore, the number of elements that can be studied using this technique is limited. One of the elements that has been studied extensively using Mössbauer spectroscopy is iron. In this work, Mössbauer spectroscopy was used to measure the fraction of iron in the Fe2+ and Fe3+ states, which can be used as a measure of the redox state of the glass sample. Mössbauer spectroscopy was also used to analyze the various iron minerals in the feed materials and deposits in the off-gas system. Mössbauer spectra were collected using an American Magnetic/Ranger Scientific MS-1200 system equipped with a 57Co source in a rhodium matrix with glass powder as the sample. Both divalent and trivalent iron show doublet peaks in the Mössbauer spectrum and the peak areas are proportional to the concentrations of the respective species in the glass. Even though the peaks overlap partially, software can be used to deconvolute the peaks and calculate the peak areas. The ratio of the areas of the Fe2+ and Fe3+ peaks is equal to the ratio of their concentrations in the glass. The redox measurements are calibrated using a set of six standard glass samples with Fe2+ contents ranging from 7 to 90% of the total iron (Fetotal). The standards include a NIST traceable Obsidian Rock (SRM 278), five standard glasses analyzed by Corning, Inc. for their redox state, and the DWPF-EA glass. The site populations provided by the fitting is mol% Fe, assuming that the recoil-free fraction is the same for each site. The NIST standard iron foil (SRM 1541) is used to calibrate the instrument and determine the zero velocity channel. Since Doppler shifts in energy are measured in Mössbauer spectroscopy, the velocity is a measure of the shift in energy; knowing the zero velocity channel therefore helps in identifying the Fe2+ and Fe3+ peaks. 17 SECTION 2.0 WASTE SIMULANT, GLASS FORMULATION, AND MELTER FEED ANALYSIS A high-manganese HLW stream was used for the present tests. This section describes the selected waste composition, corresponding simulant, and the testing to develop new glass formulations. 2.1 High Manganese Simulant Composition The Hanford Tank Waste Operations Simulator (HTWOS) model calculated the compositions of 4106 HLW batches to be processed at the WTP, which are given in the River Protection Project System Plan, Revision 6 [40]. A review of the compositions of these HLW batches shows that the total amount of manganese to be processed is 4.02E+5 kg (as MnO). The MnO concentrations in the waste batches vary from 0.37 wt% to 13.70 wt%, with 116 batches containing at least 10 wt% of MnO. The waste batch selected for testing is Number 3939 in the HTWOS run. The most abundant components in HLW Batch 3939 are Al2O3 (29.70 wt%) and Na2O (19.78 wt%), followed by MnO (13.70 wt%). The other major components in the waste batch are Fe2O3 and Bi2O3, which are present at 8.95 wt% and 4.14 wt% respectively. An evaluation of Hanford high-Mn HLW as part of the waste selection process for testing showed that the selected waste is indeed representative of high-Mn HLW in that they are all similar in their concentrations of other components such as Al, Fe, Na, etc., as illustrated in Figures 2.1- 2.3. Table 2.1 lists the composition of HTWOS waste batch Number 3939 with the minor oxides (< 0.1 wt%) removed. Removal of these minor oxides is intended to maintain a manageable number of oxides in testing. There are 23 oxide components in the abbreviated HLW composition in Table 2.1. In addition, to avoid the use of radioactive materials in melter testing, formulation of the HLW simulant excludes UO3. The final renormalized HLW simulant composition, which includes 22 oxides, is also given in Table 2.1. The simulant composition in Table 2.1 was the basis for HLW glass formulation development. Crucible melts were prepared and characterized to identify high waste loading glass compositions that meet all WTP processing and product quality requirements. Waste loadings in the HLW glass formulations were limited primarily by formation of manganese- containing secondary phases. Table 2.2 provides a recipe to produce the high manganese HLW simulant for 100 kg of waste oxides. The compositions of volatile components in the HLW are not given by the HTWOS model run; therefore, the concentrations used in previous melter testing are substituted in deriving the recipe in Table 2.2. The volatiles and their respective concentrations in g/100 g waste oxide are: carbonate (4.65), nitrite (0.012), nitrate (0.784), and organic carbon (0.026). The form of manganese shown in Table 2.1 is MnO, which was used in the first two tests; MnO was replaced with either MnO2 or MnCO3 in subsequent tests, depending on the form of manganese being evaluated. 18 2.2 Manganese Forms in Hanford HLW and Melter Feed Manganese in Hanford tank wastes can be present in multiple oxidation states, as various oxides and hydroxides, and in compounds with carbonates, oxalates, and other anions. Compilations of observed manganese forms in single and double shell Hanford tanks have identified the following: • Seven different phases: MnC2O4·2H2O (lindbergite), MnCO3 (rhodochrosite), Mn/FeO(OH), Fe,Mn oxide, Mn2MnO4, Fe2MnO4 (jacobsite), Mn/FeO(OH) [25]. • Nine different phases: MnFe2(PO4)(OH)2 (pseudolaueite), Fe1.75Mn0.25O3 (hematite- type oxide), MnC2O4·2H2O (lindbergite), MnCO3 (rhodochrosite), FeMnO4 (iron manganate), Mn2CrO4 (manganese chromium oxide), Mn1.5Cr1.5O4 (manganese chromium oxide), (Mn,Fe)3O4 (manganese iron oxide), and Fe2MnO4 (jacobsite) [26]. • Denser and dehydrated Mn phases including the Mn(IV) compound MnO2, the Mn(III) compound MnOOH, manganese spinels such as Mn2MnO4, other spinels that include Fe or Cr, and a mixed phase incorporating other metals and phosphorus [24]. Previous modeling work to predict the form of manganese in Hanford Tank waste by specifying the manganese as divalent gave an outputs of Mn3(PO4)2, Mn(OH)2, and MnCO3 [24]. Another model represented all Mn as the equivalent of MnO2 in light of the stability of MnO2 over a wide pH range in aqueous environments containing no anions except hydroxide [41]. For the majority of the previous HLW melter feed testing, MnO2 was used as the manganese source in the feed [10-16, 21-23, 29, 42, 43]; MnO was assumed to be the dominant form of manganese in the product glass based on measurements made on melter glasses [44]. In more recent tests conducted in support of HLW vitrification enhancements for ORP, MnO was used as the source of manganese [18-22, 45, 46]. The manganese content targeted in the glasses during these melter tests was less than four percent MnO, except in one test conducted to determine the effect of manganese on processing rate in which the concentration was eight percent MnO [43]. It is worth noting that the production rate achieved with the eight percent MnO targeted glass was only 750 kg/m2/day, which is well below the rate achieved for the same formulation at nominal manganese content and the WTP requirement of 800 kg glass /m2/day. For the present tests, MnO and MnO2 were selected to represent the reduced and oxidized forms of manganese species present in the waste and to provide a direct comparison of their effects. Testing was also performed with rhodochrosite (MnCO3), which was identified in the C-106 tank [24, 25]. Unlike the various mixed phase spinels that have been observed in the tank waste, these manganese compounds are commercially available in well characterized forms and in quantities suitable for producing feed for melter testing; they are therefore natural choices for the initial testing. 19 2.3 Development of Glass Formulation for High Mn HLW 2.3.1 High Manganese HLW and Glass Formulation Strategy The simulant composition in Table 2.1 is the basis for the present HLW glass formulation development. As evident from the waste composition expressed in terms of oxides, the major waste constituents, Al, Cr, Fe, Mn, and Ni are all highly compatible with spinel formation, a common liquidus phase for HLW glasses. Thus, one of the issues that is likely to limit waste loading in glasses to treat this Mn-rich HLW is spinel crystallization. As discussed above, melter testing of this Mn-rich HLW was conducted to evaluate the impact of different manganese sources on melt rate and processing. However, only MnO was used for glass formulation development because divalent Mn2+ has been determined to be the dominant valence state for manganese in borosilicate glasses [44]. The glass formulation work was aimed at development of HLW glass compositions for a high-Manganese HLW stream at a high waste loading that has acceptable product quality and processing characteristics. The approach employed small-scale tests and crucible melts to identify such high waste loading glass formulations. Properties that affect processability and product quality include glass crystallization, melt viscosity, melt electrical conductivity, PCT releases, and TCLP releases of the product glass. Since crystallization is likely to be the most constraining property in view of the high concentrations of spinel-compatible elements in the waste, all prepared glasses were screened with respect to crystallinity after isothermal heat treatment. Glasses that did not meet the crystallinity constraint were not characterized further with respect to the other properties. The final glass composition selected for melter tests were characterized with respect to all properties relevant to processing and product quality for HLW glasses [47, 48]. A total of 20 crucible melts were prepared and characterized to develop a high-Mn HLW glass formulation suitable for melter testing (Table 2.3). Results from crucible scale testing to support the selection of the candidate glass are summarized below in groups by the waste loading in the glasses that were tested. Target and XRF analyzed glass compositions are given in Table 2.3; a summary of measured properties is given in Table 2.4; measured melt viscosities and electrical conductivities are compiled in Table 2.5; PCT releases are given in Table 2.6; and TCLP results are given in Table 2.7. 2.3.2 Formulation of High-Mn HLW Glasses at 45 wt% Waste Loading Four glasses were formulated at 45 wt% waste loading with different combinations of major alkaline additives. HLW-HMn-6 with 18.3 wt% Na2O showed 2.4 vol% spinel crystals after heat treatment at 950oC for 70 hours. Addition of 4 wt% of CaO and 3 wt% of B2O3 at the expense of Na2O did not reduce the spinel crystal content in HLW-HMn-8 (Tables 2.3, 2.4). HLW-HMn-2, formulated by substitution of 2 wt% Li2O and 3 wt% SiO2 for CaO and Na2O in 20 HLW-HMn-8, showed similar amounts of spinel crystallization. HLW-HMn-4, with addition of 2 wt% K2O for SiO2 in HLW-HMn-8, did not show reduced spinel crystallization after heat treatments at all four temperatures. Overall, at 45 wt% waste loading with 1.1 wt% Cr2O3, 6.5 wt% MnO, and considerable Fe and Ni from the waste, more than 2 vol% of spinel tended to be present after heat treatment at 950oC for 70 hours in the HLW glasses investigated in this work. Consequently, formulations with lower waste loadings were investigated. 2.3.3 Formulation of High-Mn HLW Glasses at 40 wt% Waste Loading Four glasses were formulated at 40 wt% waste loading with different combinations of major alkaline additives. HLW-HMn-5 with 6 wt% Li2O showed 1.2 vol% spinel crystals after 70 hours at 950oC. When Li2O was decreased to 4 wt % accompanied by increases in Na2O and B2O3 and a decease in SiO2, the same amount of spinel was found in HLW-HMn-3. A further reduction of Li2O to 2 wt% with the addition of 3 wt% K2O did not change the spinel content after heat treatment at 950oC in HLW-HMn-1. Addition of 2 wt% K2O for Li2O in HLW-HMn-7 increased spinel crystallization slightly at all four heat treatment temperatures (Tables 2.3, 2.4). In general, the four glasses formulated at 40 wt% waste loading showed considerably less spinel than those with 45 wt% waste loading. However, the spinel contents in the heat treated glass samples were still above 1 vol% after heat treatment for 70 hours at 950oC. 2.3.4 Formulation of High-Mn HLW Glasses at 35 wt% Waste Loading High-Mn HLW glass formulations at 45 wt% and 40 wt% waste loadings showed higher than acceptable crystallization of Fe-Mn-Cr-Ni spinels. Consequently, six glasses were formulated at 35 wt% loading to reduce spinel crystallization (HLW-HMn-9, -10, -11, 12, -13, -14). At about 10 wt% K2O, 1.4 vol% spinel crystals were present in HLW-HMn-11 after heat treatment at 950oC for 70 hours (Tables 2.3, 2.4). Substituting 6 wt% Li2O and 5 wt% SiO2 for 10 wt% K2O and 1 wt% B2O3 reduced spinel crystallization to 1 vol% at 950oC in HLW-HMn-9. The spinel crystal content decreased further to 0.7 vol% at 950oC when both K2O and Li2O were used in HLW-HMn-10. However, the variations of HLW-HMn-10 at the same K2O content but different B2O3 concentration (HLW-HMn-12), or at different Li2O and V2O5 concentrations (HLW-HMn-13), or Li2O and P2O5 concentrations (HLW-HMn-14), resulted in higher spinel crystallization (1.6 vol%, 1.1 vol%, and 1 vol% spinel for HLW-HMn-12, -13, 14, respectively, after heat treatment for 70 hours at 950oC). Although the high combined concentrations of K2O and Li2O in HLW-HMn-10 were effective in decreasing spinel crystallization while still meeting the melt viscosity and electrical conductivity requirements (Tables 2.3, 2.4), the PCT releases were too high as compared to the DWPF EA glass (Table 2.4). The PCT releases did not improve significantly with additions of V2O5 (HLW-HMn-13) or P2O5 (HLW-HMn-14). Interestingly, HLW-HMn-9, with 6 wt% Li2O and no additional K2O but higher SiO2 showed PCT releases well below the requirements (Table 2.4). The higher Li2O concentration in HLW-HMn-9 (compared to HLW-HMn-10) not only increased its electrical conductivity at the melter processing temperature, but increases the potential risk for structural damage to the K-3 refractory [49]. Therefore, additional formulations 21 at 35 wt% or lower waste loadings were investigated in order to improve the glass product quality with respect to the PCT while maintaining sufficiently low spinel crystallization. 2.3.5 Formulation of High-Mn HLW Glasses at 32 wt% Waste Loading Two glasses were formulated at 32 wt% waste loading (Tables 2.3, 2.4). At this lower waste loading, spinel crystallization was generally lower, at around 0.7 vol% at 950oC for both HLW-HMn-15 and HLW-HMn-16. PCT releases were slightly lower for HLW-HMn-16 as compared to HLW-HMn-10 at similar concentrations of K2O and Li2O additions as HLW-HMn-10. However, PCT releases of HLW-HMn-15 with 1 wt% more Li2O than in HLW-HMn-9 were higher than those of HLW-HMn-9. Overall, compared to glasses at 35 wt% waste loading, the gains in property improvements from 3 wt% lower waste loading with similar glass forming chemicals (as for HLW-HMn-10 and HLW-HMn-9) were too small to warrant further investigation. 2.3.6 Formulation at 35 wt% Waste Loading to Reduce PCT Releases As described in Section 2.3.4, HLW-HMn-10 failed the PCT release requirements but other glass properties were within acceptable limits. At the same 35 wt% waste loading and with largely identical major glass forming chemicals as in HLW-HMn-10, two more glasses were formulated by adding 3 wt% ZrO2 at the expense of SiO2 and B2O3 (-2 wt% and -1 wt%, respectively) in HLW-HMn-17 or 2 wt% ZrO2 and 3 wt% Al2O3 at the expense of SiO2 and B2O3 (-4 wt% and -1 wt%, respectively) in HLW-HMn-18 (Tables 2.3, 2.4). Addition of ZrO2 or ZrO2 plus Al2O3 substantially reduced the PCT releases for both glasses (Tables 2.3, 2.4) with very small increases in spinel crystallization. HLW-HMn-20 was formulated with the same 3 wt% ZrO2 concentration as HLW-HMn-17, but contained more SiO2 (+3.5 wt%) and Li2O (+1.5 wt%) with less K2O and B2O3 (-4 and -1 wt%, respectively). PCT releases were reduced substantially as a result: the normalized B release was 1.5 g/L (Tables 2.3, 2.4), which is ~30% of those for HLW-HMn-17 and -18, and nearly one order of magnitude smaller than those for HLW-HMn-10 while maintaining less than 1 vol% spinel crystallization after heat treatment for 70 hours at at 950oC (Tables 2.3, 2.4). At a higher SiO2 concentration of 45 wt% with more Li2O (4 wt%) and no K2O, HLW-HMn-19 showed further reductions in PCT releases (Tables 2.3, 2.4) by a factor of about 3. In addition to the reduced PCT releases, spinel crystallization was similar to that in HLW-HMn-20 (< 1 vol% at 950oC for HLW-HMn-19). However, the viscosity of HLW-HMn-19 increased substantially in comparison to that of HLW-HMn-20. 2.3.7 Selection of HLW-HMn-20 Glass Formulation for Melter Testing A total of 20 new formulations were developed and tested to identify a glass composition to treat the high-Mn HLW (Tables 2.3, 2.4). As discussed in this section, the formulation development focused on two main issues: spinel crystallization and PCT releases. The Mn-rich HLW selected for this work contains large amounts of spinel-prone constituents. As a result, the waste loadings are primarily constrained by Cr-Mn-Fe-Ni spinel crystallization. Addition of 22 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 fluxes (like alkalis, alkaline earths, boron, etc.) to the glass formulations tended to reduce spinel crystallization, but also increased PCT releases. The formulation development work therefore had to manage these competing factors. Based on the results obtained, HLW-HMn-20 was selected as the best formulation for melter testing because of its acceptable processing properties (crystallinity, viscosity, electrical conductivity) and product quality (PCT and TCLP releases). Another formulation, HLW-HMn-19 with higher Li2O content, showed similar glass properties except for higher melt viscosity. HLW-HMn-19 was not selected for further testing because higher melt viscosity tends to reduce feed processing rates, and, more importantly, previous work has indicated a higher risk of structural damage to K-3 refractory in glasses with more than about 4 wt% Li2O [49]. The formulation HLW-HMn-20 meets all of the processing and product quality requirements, as summarized in Table 2.8. At 35 wt% waste loading with almost 0.9 wt% Cr2O3, HLW-HMn-20 showed 0.9 vol% spinel crystals after heat treatment for 70 hours at 950oC. Images of the heat treated glass samples are shown in Figure 2.4. The measured values of glass melt viscosity and electrical conductivity (see Table 2.5) are within acceptable ranges for the WTP. The PCT releases for HLW-HMn-20 are an order of magnitude lower than those for the DWPF-EA glass (see Table 2.6). The PCT releases of the CCC sample of HLW-HMn-20 are very similar to those of the quenched sample. TCLP releases of glass HLW-HMn-20 are well below the delisting limits (see Table 2.7). The recipe for the melter feed, which includes the waste simulant and additives, to produce 100 kg of glass (with MnO as the manganese source) is given in Table 2.9. 2.4 Analysis of Melter Feed Samples 2.4.1 General Properties Feed samples from as-received drums without manganese were analyzed to confirm physical properties and chemical composition. The measured solids content of the as-received feed samples along with the amount of manganese to be added were used to calculate the amount of water required to achieve the target solids content for each feed. Before the addition of manganese to the as-received melter feed, the measured solids content was about fourteen percent above the target glass yield; thus, water was added to adjust the solids content of the as-received feed as well as to compensate for the solids added as the manganese source. Melter feed samples were also taken during each melter test from either an in-line sampling port or directly from the feed tube at the end of a test. Sample names and measured properties are given in Table 2.10. Density, pH, water content, glass conversion ratio, and oxide composition by XRF and DCP-AES were measured on the samples. The measured glass conversion ratios for all feed samples from the melter tests were within two percent of the target on a weight-per-weight basis, validating the use of the target conversion ratio for calculating glass production rates. The water content, density, glass yield, and pH varied within very narrow ranges for the melter feed test samples; no significant difference in these measured properties was discernable for feeds with different manganese sources. The pH of the as-received feed was essentially the same as the melter test feed, indicating that the various manganese sources added had no effect on the pH of the feed, as would be expected. 23 2.4.2 Chemical Composition The methods used for analysis of the chemical compositions of feed samples are described in Section 1.4.2. The boron and lithium oxide concentrations from the DCP-AES analysis were used for normalizing the XRF data since their concentrations were not determined by XRF. The analyzed compositions of the as-received feed and feed sampled during melter tests are compared to the target compositions in Tables 2.11 and 2.12. The results for the as-received feed samples without manganese show good agreement with the target composition for most of the constituents; all oxides with concentrations greater than one weight percent show deviations from target of less than ten percent except for lithium, which is less than thirteen percent. Also of note in the analysis of the as-received feed is that no manganese was detected, as intended. The average analysis of the feed for melter tests approximated the target composition with all of the constituents with target concentrations greater than one percent deviating by less than about ten percent, including manganese, which was only about three and a half percent below the target concentration. Average analyzed boron and lithium concentrations for melter test feed samples were 7.38 and 10.07 percent below target concentrations, and therefore this feed sample analysis instead of the target values was used to normalize XRF values in product glasses. Depletions of the volatile minor components sulfur and thallium were observed due to loss during the crucible melting procedure. Low concentrations (up to 0.04 %) of chlorine, titanium, and zinc in the feed samples were detected, even though they were not included in the target composition, presumably originating from trace level contamination of feed additives and chemicals used to produce the waste simulant; this is not expected to have any significant impact on the glass or processing properties of the melter feed. 2.4.4 Vertical Gradient Furnace The vertical gradient furnace has been used as a useful screening tool for ranking HLW slurry feeds for their processing rate [16, 21, 22, 27-29]. Melter feed samples from each of the three tests with different forms of manganese, all producing the same HLW-HMn-20 glass composition, were tested under the standard VGF conditions in an attempt to evaluate the potential impact of the form of manganese on melt rate. Aliquots from one liter sized slurry feed samples were dried and subjected to the test protocol described in Section 1.4.1. The chemical compositions of the sampled feeds are given in Table 2.12. Additional tests were performed on samples produced at the crucible scale on the HLW-HMn-10 composition (see Tables 2.3 and 2.4) to evaluate the effect of added reductant to feed containing MnO 2. In a standard VGF experiment, feed samples are examined for the extent of feed reactions, melting, appearance of the feed sample such as the presence of foam, formation of a dome-like structure, etc., that are indicative of the rate of feed conversion to glass. The conversion of each type of feed material was evaluated primarily based on images of the top and cross sections of the reacted feed samples after 15, 30, and 60 minute VGF tests, depending on the observed completion of reactions. The top and cross sectional images of VGF samples are shown in Figures 2.5 – 2.8. A summary of the visual observations and relative rankings of the feeds are compared to the previously tested HLW-NG-Fe2 composition with various forms of iron [16, 29] in Table 2.13. 24 The two feeds with divalent manganese (MnO and MnCO3) from the present tests were quickly converted to glass, earning the highest ranking for feed conversion using the VGF method. The feed conversion with more oxidized manganese (MnO2) was considerably slower with a thick foamy layer on the wall of the reaction vessel after 30 and 60-minute VGF tests, resulting in a ranking of 3. Typically, formation of such a thick layer that is full of gas vesicles indicates episodes of degassing, foaming, and subsequent collapsing of an over-arching dome structure, resulting in the overall conversion rate from melter feed to glass being slower. Previous tests with the high iron HLW-NG-Fe2 composition did not show differences in melt rate with different iron oxidation states; both ferrous and ferric oxides resulted in rapidly melting feeds. The carbonate associated with MnCO3 did not have an effect on the observed melt rate. In previous tests, the hydroxide form of iron resulted in slower melt rates than the oxide form, in contrast to aluminum hydroxide, which resulted in faster melt rates than aluminum oxides [27]; therefore, it is difficult to predict whether feeds with manganese hydroxide would melt faster than the oxides tested in the present work. In addition to the tests with melter feed samples, HLW-HMn-10 at 35 wt% waste loading was subjected to feed conversion tests to assess its processing rate and potential impact due to different Mn chemical forms. Very similar VGF results were obtained for the HLW-HMn-10 formulation as for the feed samples from the melter tests: feed samples reacted fast with MnO and MnCO3, but slower with considerable foam with MnO2 (Figure 2.8). The observed porous structures in VGF samples of the MnO2-sourced HLW-HMn-20 and HLW-HMn-10 formulations were probably caused by redox reactions of manganese during feed conversion. As identified from structural analysis of Mn-bearing glasses, MnO is the dominant form of manganese in HLW glasses quenched from melter processing temperature (1150oC) [44]. Therefore, it is expected that the MnO2 present in melter slurry feed would be reduced to MnO with a concomitant release of oxygen gas. The observed foaming was likely the result of the oxygen gas trapped within a viscous fluid formed from the partially molten feed blend. One effective method to suppress undesirable foaming during melter processing is to add a reductant to the slurry feed. In the WTP low activity waste (LAW) flow-sheet, sugar (sucrose) is used for this purpose. Therefore, the addition of sugar was investigated with respect to its effects on feed reactions in the HLW-HMn-10 formulation with MnO2. Two feed samples were tested with two levels of sugar in the feed formulation. One feed sample was prepared with an amount of sugar corresponding to the 0.5 carbon-to-nitrate stoichiometry, which is the baseline for mitigation of foaming in high-nitrate LAW feeds [50]. Using this basis, for each mole of MnO2 in the feed, approximately 0.02 moles of sugar was used. This corresponds to about half of the stoichiometric amount of carbon required to convert into CO2 all of the oxygen generated from the decomposition of the MnO2 to MnO. In the second feed, twice this amount of sugar was added. Foaming, similar to that observed in the MnO2-sourced feed samples, developed for the feed with 0.5 stoichiometric carbon. However, at twice that sugar content, the feed reacted very fast and completed conversion with no sign of foaming, very similar to the MnO-sourced feed of the same HLW-HMn-10 formulation. These results indicate that the addition of a reductant at a sufficient level is effective in suppressing foaming due to the reduction of MnO2 during feed conversion. 25 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 SECTION 3.0 DM100 MELTER OPERATIONS Melter tests were conducted on the DM100-BL vitrification system between 11/14/16 and 12/2/16 with the high manganese, HTWOS Model Run Waste Batch 3939 HLW simulant and the HLW-HMn-20 glass composition. These tests produced nearly 900 kilograms of glass from nearly two and half metric tons of feed. Feed for the tests was obtained in a single batch without manganese and MnO, MnO2, or MnCO3 was added to the test batch depending on the form of manganese being tested. In all tests, the glass temperature was held constant at 1150°C, the feed solids content was constant at 500 g glass per liter feed, and the waste oxide and glass compositions were identical. Melt pool bubbling was held constant at 9 lpm for tests with each of the manganese forms; the bubbling rate was optimized during the first test with MnO in order to facilitate compositional turnover of the melt pool prior to testing each of the forms of manganese at nominal bubbling conditions. This testing protocol permitted the determination of the effects of the form of manganese on production rate and processing properties and facilitated comparison with previously conducted tests. Attempts were made to replicate the melter configuration and operating conditions used for previous tests with HLW simulants [3, 11-17, 20-23, 27-29, 32, 33, 45, 46]. These conditions include a near-complete cold cap, which is between 80-95% melt surface coverage for the DM100 since a 100% cold cap tends to lead to "bridging" in smaller melters. Summaries of the tests are provided in Table 3.1. The series of four nominally 50-hour tests were divided as follows: • MnO as the manganese source, optimized bubbling • MnO as the manganese source, nominal bubbling • MnO2 as the manganese source, nominal bubbling • MnCO3 as the manganese source, nominal bubbling. The feed and glass were processed without significant difficulties throughout the majority of the tests. Cold cap conditions were similar to the range of conditions observed in previous tests with HLW feeds [3, 11-17, 20, 27, 32, 33]. The feed formed some shelves along the walls of the melter, although not to the rate-limiting extent observed while processing some high aluminum formulations [3, 28] or some high iron formulations [23] except during portions of the test with feed containing MnO2. Manual methods were used to dislodge these deposits without any interruptions in feeding after discharging glass, which lowered the glass level in the melter leaving deposits adhering to the walls out of contact with the molten glass. Feed with manganese carbonate required the least amount of deposit removal but did not process at the fastest rate of the three feeds with different forms of manganese. Occasionally, liquid would pond on the cold cap surface and abruptly flow to the melt pool surface causing minor excursions in melter 26 pressure. Short, routine interruptions were required during testing to transfer feed to the feed tank. No foam was observed on the melt pool surface or cold cap and no foamy glass was observed in the glass discharge. Glass production rates as moving hourly and cumulative averages while processing the HLW-HMn-20 glass composition and three different manganese sources are illustrated in Figures 3.1.a - 3.1.d. The cumulative average rates approximate the steady state processing rates for all four tests as a result of the consistent operation over the course of each test except during the latter portion of the test with feed containing MnO2 where excessive shelves and ridges formed. Production rates achieved while processing the HLW- HMn-20 composition exceeded WTP processing rate requirements in feeds with MnO as the manganese source, but were lower than those measured for other HLW compositions whose processing rates have been optimized at VSL in work for ORP. Steady state production rates for present and previous tests [16, 17, 20-22, 27, 32] conducted at 9 lpm fixed bubbling and optimized bubbling with glass formulations optimized for a range of HLW compositions are tabulated in Table 3.2. As compared to the 800 kg/m 2 /day baseline rate for the WTP HLW vitrification system, the production rate for the P P present high manganese waste under nominal conditions is 15 percent higher with MnO, 7 percent lower with MnO2, and equal with MnCO3. The achieved production rates at nominal conditions are also below the range of 1100 to 1900 kg/m 2 /day for the HLW streams with P P optimized glass formulations that have been tested previously. Bubbling optimization did, however, result in a production rate increase of 70 percent, bringing the rate to 1560 kg/m 2 /dayP P when processing feed with MnO as the manganese source. Production rates for the HLW-HMn-20 glass composition with various forms of manganese and HLW-NG-Fe2 glass composition with various forms of iron [16, 29] conducted with the same operating conditions and feed solids content are compared in Table 3.3 and depicted in Figure 3.1.e. Feeds with the manganese sources tested resulted in steady state production rates ranging from 750 to 920 kg/m 2 /day and trended as follows: P P MnO2 < MnCO3 < MnO The lowest production rate was associated with feed containing MnO2 as the manganese source, in agreement with VGF testing, which indicated that feed with MnO2 melted slower than feeds with other manganese sources (Section 2.4.4). VGF testing also indicated that feeds with HLW-HMn-20 glass composition using either MnO or MnCO3 as the manganese source were rapidly melting; however, relatively low production rates of 800 and 920 kg/m 2 /day were P P obtained during melter testing. By comparison, for the HLW-NG-Fe2 glass composition, VGF testing showed the feeds to be rapidly melting, in agreement with results from melter testing, which gave production rates from 1725 to 1950 kg/m 2 /day [29]. Contrary to the trend observed P P with manganese, slower processing rates were not observed for the more oxidized forms of iron for which the melter processing rates were in the order: Fe(OH)3 < Goethite (FeOOH) < Magnetite < Hematite < NOAH iron mixture Comparison of the two trends indicates that the transition metal oxidation state and mineral forms for specific waste components have unique effects on melter feed processing rates 27 and caution should be exercised in extrapolating trends for one waste element to another. Similar observations were made in the comparison between various iron and aluminum forms in the waste [28]. The relative magnitude of processing rate change in response to changes in forms of iron and manganese is compared in Table 3.3. The magnitude of the processing rate change with manganese form ranged from 120 to 170 kg/m2/day or a 13 to 18% decrease over MnO. This level of difference is comparable to that observed between some of the iron forms on an absolute basis; however, on a percentage basis the differences are twice as high for the manganese forms, due in part to the lower overall production rates with HLW-HMn-20 composition. The effect of manganese form on production rates is even more pronounced when considering the manganese oxide content in the glass is only about five weight percent, as compared to the iron oxide concentration of about sixteen weight percent in the HLW-NG-Fe2 composition. The results of various operational measurements that were made during these tests are provided in Table 3.4. Glass temperatures are shown in Figures 3.2.a and 3.2.b, plenum temperatures in Figures 3.3.a and 3.3.b, electrode temperatures in Figures 3.4.a and 3.4.b, glass resistance in Figures 3.5.a and 3.5.b, melt pool bubbling in Figures 3.6.a and 3.6.b; electrode power is included in the figures with electrode temperatures and glass resistance. Bulk glass temperatures measured at 5 and 10 inches from the bottom of the melt pool averaged within 6°C and 13°C of the target glass temperatures of 1150°C, respectively, during each of the four tests. Glass temperatures closer to the top of the melt pool (measured at 16 and 27 inches from the bottom) averaged up to 21°C lower and are not as reliable indicators of bulk glass temperatures as a result of their sensitivity to variations in the level of glass in the melter and gradients near the melt surface. Downward spikes in glass temperature, particularly around the top of the melt pool, are often observed in response to glass discharging. The discharge chamber temperature was maintained above 1000°C over the course of the tests to facilitate pouring of the glass product. On average, the upper and lower electrode pairs were about 100 to 200ºC colder than the glass pool over the course of the tests. The bottom electrode, which was not powered, was about 200ºC to 300ºC colder than the powered side electrodes. Plenum temperatures ranged mostly from 400°C to 500°C, indicative of a complete cold cap during steady state processing. Higher plenum temperatures were measured at the beginning of testing during the development of the cold cap. Plenum temperatures measured in the thermowell were periodically up to 15°C lower than those measured by the exposed thermocouple, depending on the extent of direct exposure to the glass surface. The target bubbling rate of 9 lpm was maintained in each of the three tests conducted at nominal conditions. The feed rate was maximized by increasing bubbling to 15 lpm during the initial test. Power supplied to the electrodes averaged from 17.9 to 26.0 kW and increased with increasing production rate: the test with optimized bubbling maximizing production rate averaged 26.0 kW power use as compared to 17.9 to 19.1 kW power use for tests conducted at nominal bubbling. The average power usage normalized to glass production rate was relatively low at 3.9 kWhr/kg for the test with optimized bubbling and higher 4.6 – 5.2 kWhr/kg for tests conducted with nominal bubbling because much of the supplied energy is used to maintain the glass pool at the target melt temperature (i.e., the essentially constant idling power); thus higher production rates result in relatively lower normalized power usage. At the onset of testing, the 28 glass pool resistance increased from 0.045 to 0.11 ohms as the melt pool fully reached the target glass composition. Subsequently, melt pool resistance was relatively constant between 0.104 and 0.113 ohms as a result of the lack of compositional change, uniformity of melt pool bubbling, and the constant glass pool temperature of 1150°C. The gas temperature at the film cooler averaged around 278ºC during the tests and depended on the plenum temperature, the amount of added film cooler air, and the temperature of the added film cooler air. The high temperature is maintained in order to prevent condensation in the downstream filtration units. Drops of around fifteen degrees in gas temperature were observed across the (insulated) transition line for three out of the four tests. 29 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 SECTION 4.0 GLASS PRODUCT ANALYSIS Nearly nine hundred kilograms of glass was produced in these tests. The glass was discharged from the DM100 melter periodically into 5-gallon carbon steel pails using an air lift system. The discharged product glass was sampled by removing sufficient glass from the top of each pail for total inorganic analysis. Product glass masses and discharge date are given in Table 4.1. Glass samples were also taken by inserting a threaded metal rod directly into the glass pool. These “dip” samples serve to document the composition of the glass pool before and after testing. No macroscopic secondary phases were observed in any of the discharged glasses or dip glass samples. 4.1 Compositional Analysis of Discharge and Dip Glass Samples All discharge glass samples were crushed and analyzed directly by XRF. Since boron and lithium are not determined by XRF, boron and lithium concentrations were calculated from the average measured feed sample concentrations, the initial concentrations measured in the melt pool, and the nominal glass volume of the melter. All dip glass samples were also analyzed by XRF and dissolved for DCP-AES determination of boron and lithium. The analyzed compositions of discharged and dip glass samples are provided in Tables 4.2 - 4.5. A comparison of the target composition and the analyzed terminally discharged glass from each test is provided in Table 4.6. The analytical results from samples at the end of testing compare favorably to the target values and feed sample analyses (see Section 2.4.2). All oxides measured by XRF with a target concentration greater than one weight percent showed less than 10% deviation from the target values for the terminal test, which used MnCO3 as the iron source. Surpluses of phosphorus and deficits of potassium and zirconium for glasses from the end of tests processing feeds with MnO and MnO2 resulted from incomplete turnover of the melt pool before and during the tests. Manganese oxide concentrations averaged within eight percent of the target in the nominally conducted tests with the three forms of manganese. The measured boron and lithium concentrations in the dip samples were very similar to those in the feed sample analysis validating the use of average feed sample analysis to calculate boron and lithium concentrations for discharge glasses. Chlorine, titanium, and zinc were measured in the product glass at low concentrations despite not being included in the target composition as a result of their presence in the feed as contaminants. Depletions of volatile minor components, chromium, fluorine, sulfur and thallium, were observed due to loss during the vitrification process. Compositional trends for selected constituents shown in Figures 4.1.a - 4.1.g illustrate the approach of the majority of the glass constituents to the target composition over the course of the tests. The composition of the glass pool at the beginning of the test was from a previous test with a high phosphate HLW [51], which contains significantly more sodium, phosphate, and iron than the HLW-HMn-20 composition with less than one weight percent manganese oxide; therefore, 30 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 the composition of the glass pool changed dramatically over the course of the tests. Changes in glass pool composition are observed as increases in the concentrations of manganese, silicon, potassium, lithium, zirconium, thallium, and lanthanum at the expense of aluminum, sodium, iron, bismuth, phosphorus, calcium, and sulfur during the transition to the HLW-HMn-20 composition. The majority of the compositional change occurs during the initial segment of the test, although some changes in potassium, manganese, iron, phosphorus, and zirconium occur over the subsequent test as a result of the difference in composition between the glass pool composition at the start of testing and the HLW-HMn-20 composition. The most apparent compositional changes are the increases in MnO concentration from less than one to nearly five weight percent; increases in K2O concentration from about half to four weight percent; decreases in Na2O concentration from over twenty to about seven weight percent; and decreases in P2O5 from seven to one weight percent. Minor oxides, lead, nickel, magnesium, chromium, neodymium, and strontium, were relatively constant in concentration over the course of the tests. Fluorine and thallium reach only about a third of their respective target concentrations and sulfur reaches only about half the target due to volatilization from the glass pool and cold cap. 4.2 Chemical Durability of Discharge Glasses Samples of glass discharged from the end of the DM100 tests produced while processing feed with each of the three manganese forms were evaluated for chemical durability using the PCT and TCLP methods. The PCT results are compared to those for the benchmark DWPF-EA glass and the comparable crucible glasses in Table 4.7; the TCLP results are compared to the WTP delisting limits [52, 53] and Universal Treatment Standard (UTS) limits in Table 4.8. Additionally, the concentrations of manganese were measured in the TCLP leachates as a point of comparison between the glasses since there are no regulatory limits for manganese in the TCLP procedure. The chemical durability determined for the melter glass by both of these methods is excellent. All measured normalized PCT releases for the discharge glass samples are more than an order of magnitude lower than the corresponding values for the DWPF-EA glass. All regulated TCLP leachate concentrations are less than half a mg/l and below the WTP delisting and UTS limits. Measured PCT releases for melter glasses were lower than those for crucible glasses due perhaps to higher than target concentration of silica and lower than target concentrations of boron in the melter glasses. No obvious trends in PCT release are observed in the melter glasses generated from feeds containing the different forms of manganese. Comparison of TCLP results amongst the various glasses shows little variability in chromium, minor variability in nickel and manganese, and significantly less lead for the crucible melt than for the melter glasses. Higher lead concentrations may be attributable to higher concentrations in the melter glass due in part to the higher concentrations in the melter glass at the onset of testing. The chemical durability of these glasses is generally within the range measured on glasses produced from wastes limited by bismuth, chromium, aluminum, and aluminum plus sodium [3], chromium and iron [20, 16], phosphorus [32], strontium [21], and zirconium [22]. These results confirm that glasses can be formulated with higher manganese contents and meet glass product quality requirements. 31 4.3 SEM and Mössbauer Analysis of Melter Glass Samples Discharge and dip glass samples from the end of tests processing each form of manganese were subjected to XRD and Mössbauer analysis to determine the secondary mineral content and iron oxidation state. Additional SEM analyses were performed on discharge glasses from the end of tests processing each form of manganese. The results are summarized in Table 4.9 and detailed descriptions of observed mineral phases are given in Table 4.10. The amount of crystalline phases detected in samples analyzed by both XRD and SEM were very similar with no clear bias for a given method in keeping with previous tests with high chromium wastes [54]. No traces of the manganese minerals present in the feeds, manganosite (MnO), pyrolucite (MnO2), and rhodocrosite (MnCO3), were detected in any of the glass samples. No spinels and minimal divalent iron was detected in the glass pool at the start of testing. The amount of spinels detected in samples over the course of the tests ranged from 0.6 to 1.1 volume percent. The amount of divalent iron ranged from none detectable to 4.4% of total iron at the end of testing indicating oxidizing conditions in the melt throughout the tests. Marginally higher concentrations of spinels were detected in the discharge than dip glass samples presumably due to the slower cooling history of the discharge glass samples. Marginally higher concentrations of divalent iron were often detected in dip samples as compared to contemporaneous discharge glasses. No clear distinctions can be made between the amounts of crystalline phases in glasses produced from feed with the different manganese sources. The crucible melt glass for this composition contained 0.5 volume percent spinels (1 wt% see Table 2.4), which is less than that in any of the glasses from the melter tests. The higher crystal content measured in samples from melter testing may be attributable to an increased tendency to form crystalline phases due to potentially slower cooling in the larger discharge containers as compared to the crucible, differences in redox state of the melter glass versus the crucible glass, potential carryover of small amounts of crystals from the melter bottom, or slightly higher iron concentrations in the melter glasses. The crystalline phases observed by SEM were spinels containing iron, manganese, nickel, and chromium, similar to those observed in tests with a high iron HLW composition [29] and high chromium HLW composition [54]. Those tests showed that the amount of spinels in the product glass is not largely affected by the form or oxidation state of iron or chromium but the balance of reductants (organic compounds) and oxidants (nitrates and nitrites) in the melter feed. The high manganese simulant processed in the present tests contained very little organic carbon, which would limit the amount of reduced iron and its tendency to increase spinel formation. 32 SECTION 5.0 MONITORED OFF-GAS EMISSIONS 5.1 Particulate Sampling The melter exhaust was sampled for metals/particles according to 40-CFR-60 Methods 3, 5, and 29 at steady-state operating conditions during each test segment. The concentrations of off-gas species present as particulates and gaseous species were derived from laboratory data on solutions extracted from air samples (impinger solutions, filters, and rinse solutions) together with measurements of the volume of air sampled. Particulate collection required isokinetic sampling, which entails removing gas from the exhaust at the same velocity that the air is flowing in the duct (40-CFR-60, Methods 1-5). Typically, a sample size of 30 dscf was taken at a rate of between 0.5 and 0.75 dscfm. Total particulate loading was determined by combining gravimetric analysis of the standard particle filter and chemical analysis of probe rinse solutions. An additional impinger containing 2 N NaOH was added to the sampling train to ensure complete scrubbing of acid gases. The collected materials were analyzed using direct current plasma atomic emission spectroscopy for the majority of the constituents and ion chromatography (IC) for anions. Melter emission fluxes are compared to feed fluxes and emission samples taken while processing the same glass compositions in Table 5.1. Notice the distinction that is made between constituents sampled as particles and as "gas". The "gaseous" constituents are operationally defined as those species that are scrubbed in the impinger solutions after the air stream has passed through a 0.3 µm heated filter. All samples were well within the 90 - 110% limits for isokinetic sampling. Particulate emissions while processing the HLW-HMn-20 glass composition with MnO constituted from 0.23 to 0.34 percent of feed solids for the optimized bubbling and fixed bubbling tests, respectively. These levels of carryover are considerably lower than the range measured while processing various feeds containing high iron HLW simulants processed on the same melter at a temperature of 1150oC: AZ-102 (0.57 - 1.47 percent) [15]; C-106/AY-102 SIPP (0.61 to 0.81 percent) [12]; the former C-106/AY-102 baseline (0.3 - 0.74 percent) [42]; the C-106/AY-102 high waste loading formulation (0.66 and 0.71 percent) [16]; high chromium HLW-HCr-16 formulation (0.70 and 0.62 percent) [20]; high strontium HLW-HSr-7 formulation (1.14 and 0.58 percent) [21]; high zirconium HLW-ZrA-07 formulation (1.57 and 2.51 percent) [22]; high zirconium HLW-Zr-11 formulation (3.05 and 1.77 percent) [22]. However, the emissions from the present tests were within the range of measured carryover for previous tests with chromium, bismuth, aluminum, and aluminum plus sodium limited HLW wastes (0.04 – 0.57) [3, 27, 28], high bismuth HLW-Bi-F3 formulation (0.30 and 0.39 percent) [17], high phosphate HLW-HP-16 composition (0.34 and 0.23) [32], and high bismuth HLW-Bi-F9 formulation (0.18 percent) [17] when processed under the same melter conditions. Carryover is a function of the composition of the feed, particularly the amount of volatile constituents in the feed, and the conditions in the melter, particularly the completeness and uniformity of the cold cap. The relatively low particulate carryover in the present tests, the tests with high bismuth 33 formulations [3, 17], and the tests with high aluminum formulations [3, 26, 27], and high phosphate [32] were a result in part of the low volatile content of the feed. Much higher levels of carryover were observed in tests with higher amounts of volatile constituents such as rhenium, cesium, and chlorine, which are emitted primarily as fine particulate [55]. Two of the volatile constituents in the HLW-HMn-20 composition, fluorine and sulfur, are emitted in larger proportion as gaseous species and therefore do not contribute as significantly to the calculated carryover of feed solids. Also the two most volatile constituents in the HLW-HMn-20 feed, fluorine and thallium, are targeted in the glass at 0.09 wt% or less and therefore have a limited effect on the overall total particulate carryover. Increases in particulate carryover, 0.23 vs. 0.34 percent, were observed with increases in bubbling rate, in keeping with several previous tests processing HLW compositions [3, 10, 11, 16, 20-22]. Carryover values for tests conducted with the nominal bubbling rate with each manganese form ranged only from 0.23 to 0.3 percent of feed solids indicating that the form of manganese in the melter feed has little effect on the amount of particulate carryover. The composition of the particulate in the melter exhaust is reflective of the feed composition, with some enrichments or depletions based on elemental volatility. Elements present in the particulate at a proportion lower than in the feed are aluminum, silicon, nickel, phosphorus, and zirconium, while boron, chromium, alkalis, lead, fluorine, thallium, and sulfur were emitted at rates considerably higher than that for the total particulate. Other elements, including manganese, were emitted at similar rates to the overall solids carryover rate. The highest carryover was clearly observed for the most volatile elements, thallium, sulfur, and fluorine, as expected. No difference in these trends was observed with the changing form of manganese over the course of the tests indicating that the relative carryover of manganese is not affected by the mineralogy or grain size of the different forms of manganese. Boron, fluorine, and sulfur were the only elements detected in the impinger solutions collected downstream of the heated particle filter in the sampling train, which constitutes the “gas” fraction of the melter emissions. 5.2 Particulate Sampled from Off-Gas System The amount of material accumulated in the cyclones downstream of the film cooler is listed in Table 5.2. The amount of material removed from the cyclones accounts for less than a tenth of a percent of the feed solids from the tests. This is lower than the amount of particulate sampled in the melter exhaust, suggesting that some of the particulate is too fine to be removed in the cyclone or solids are deposited in the line in between the exhaust sampling point and the cyclone. The analyzed mineral content and chemical composition of material accumulated in the cyclones is provided in Tables 5.2 and 5.3, respectively. Cyclone solids contain all of the feed components in similar proportions to the feed for most elements with significant enrichments over feed for volatile elements boron, thallium (12-16 times), and sulfur (4-6 times) as well as a twofold depletion of silicon. These proportions of volatile and non-volatile elements in the cyclone particulate indicate bulk carryover of feed from the melter coupled with the loss of the most volatile components from glass pool and cold cap. The enrichment of thallium and sulfur in the cyclone deposits confirms the high measured elemental carryover in the melter exhaust (see Table 5.1). The results from XRD analysis show that most of the mineral phases detected in the 34 cyclone deposits were present in the feed as either additives (quartz and zircon) or waste components (eskolite, manganosite, and pyrolucite), suggesting direct entrainment of feed components into the melter exhaust stream. It is worth noting that the mineral form of manganese in the cyclone deposits matches the form fed for the respective test. Also no rhodocrosite (MnCO3) was detected in the cyclone deposits, suggesting that the carbonate decomposes at lower temperatures than the two oxides. The hematite detected in the cyclone deposits originates from the Fe(OH)3 in the waste simulant. 5.3 Gases Monitored by FTIR Melter emissions were monitored in each test for a variety of gaseous components, most notably CO and nitrogen species, by Fourier Transform Infra-Red Spectroscopy (FTIR). The off-gas system temperature is maintained well above 100°C beyond the sampling port downstream of the DM100 HEPA filter to prevent analyte loss due to condensation prior to monitoring. The data, therefore, represent the relative concentrations of volatile gaseous species in the melter exhaust. A summary of the range and average concentrations of gaseous species monitored during the tests is provided in Table 5.4. The analytes listed in Table 5.4 are those that were thought likely to be observed during the tests based on previous work; no other species were detected in the off-gas stream by FTIR. The concentrations of the most abundant monitored species, nitrogen monoxide, carbon dioxide, and water, are plotted in Figures 5.1.a - 5.1.c. Generally, emissions from the DM100 were relatively low as a result of the low concentrations of nitrogen, organic carbon, and ammonia in the feed. The most abundant nitrogen species monitored was NO, which is in keeping with previous melter tests with both HLW and LAW feeds. The concentrations of the most abundant measured species, water and carbon dioxide, increased with the feed processing rate since the feed water and carbon content were nominally constant for all feeds except for the last test with MnCO3, which showed higher concentrations of carbon dioxide. Carbon monoxide and ammonia were detected only in the test with MnCO3, which also had NO concentrations about three times less than in the other tests; the reason for this is not clear but it may indicate that the MnCO3 has trace level contamination of organic carbon. The scatter in the emissions data over the course of the tests is due in part to changes in the cold cap. 35 SECTION 6.0 SUMMARY AND CONCLUSIONS This report describes the results from work performed to develop and test new glass and feed formulations in order to increase waste loading for HLW with high concentrations of manganese. A further objective of the work was to determine the effect of the form of manganese in Hanford HLW on feed processing rates. A number of HLW batches to be processed at the WTP have manganese concentrations that extend above about thirteen weight percent on an oxide basis. These high manganese HLW streams frequently contain significant amounts of chromium, iron, and nickel, which when combined with manganese have the tendency to form secondary phases such as spinels that can limit waste loading or lead to poor cold cap behavior and slow processing rates [23]. Previous studies for ORP have explored some of the HLW streams that contain relatively high concentrations of iron and chromium with manganese [23]; however, these studies did not focus on HLW streams for which glass waste loading is manganese limited. Manganese is present in Hanford tank waste in a variety of forms including MnO, MnO2, MnCO3, spinels and hydroxides with iron and nickel, and oxalates [24-26]. These differences in manganese form have the potential to affect waste and melter feed rheology, feed processing rates, and the extent of crystalline phases in the glass product, as has been observed with different forms of aluminum and iron in HLW waste simulants [27-29]. In particular, glass formulation development for high manganese HLW can be challenging due to spinel formation, especially in the presence of other spinel forming elements such as iron, chromium, and nickel [6, 12, 23, 30]. In addition, foaming of the glass pool during vitrification has been attributed to manganese oxidation state changes [13-15] and this may also be affected by the form of manganese in the waste. These issues were addressed by developing glass formulations for a Hanford HLW stream with high concentrations of manganese followed by melter testing with the selected glass composition with feed containing manganese in three different forms likely to be present in Hanford tank waste. The work included preparation and characterization of crucible melts to evaluate the effects of waste loading on glass properties and the maximum waste loadings that can be achieved. The results from crucible-scale testing supported subsequent DM100 melter tests designed to further assess the enhanced glass and feed formulations with respect to processing rate and product quality. The DM100-BL, which is one of two DM100 melter systems installed at VSL, was selected as the platform for these tests due to its extensive previous use in processing rate determination for various HLW streams and glass compositions [3, 11-17, 20-23, 27-29, 33, 42, 43, 45, 46]. A strategy similar to that employed successfully for determining the differences in the feed and glass properties and feed processing characteristics of HLW feeds with different forms of aluminum and iron [27-29] was used for the present tests with different forms of manganese. Twenty glass formulations were prepared and characterized to identify a high waste loading glass composition to treat the present high-Mn HLW. Crystallization of spinel was 36 expected to limit waste loading in glasses formulated for this HLW, because, in addition to Mn, this HLW contains high concentrations of components such as Al, Cr, Fe, and Ni that can promote spinel formation. Accordingly, initial glass formulation efforts were aimed at limiting spinel crystallization by increasing the amount of components such as alkalis, alkaline earth oxides, and boron oxide in the glass composition. All of the glasses formulated at waste loadings of 45 and 40 wt% crystallized more than one vol% spinel after heat treatment for 70 hours at 950ºC. Varying the concentrations of glass former additives Li2O, K2O, Na2O, CaO, B2O3 and SiO2 did not reduce spinel crystallization to less than one volume percent in these glasses. Subsequently, glasses were formulated and tested at waste loadings of 35 and 32 wt%. At these lower waste loadings, spinel crystallization could be limited to less than one vol% after heat treatment for 70 hours at 950ºC. Glass HLW-HMn-10 formulated at 35 wt% waste loading with 2.0 wt% Li2O and 8.22 wt% K2O as additives showed acceptable crystallization, melt viscosity and melt electrical conductivity, but failed the PCT release limits. This issue was addressed in glass HLW-HMN-20 by increasing Li2O (to 3.5 wt%) reducing K2O (to 4.22 wt%), adding ZrO2 (3.09 wt%), and increasing SiO2 and Al2O3 concentrations. As shown in Table 2.8, glass HLW-HMN-20 meets all of the WTP processing and product quality requirements and was, therefore, selected for further testing on the DM100 melter to determine its processing characteristics. Melter tests were conducted on the DM100 with the new HLW-HMn-20 glass formulation using the Batch 3939 high-manganese HLW simulant. Tests on the DM100 were conducted at 1150oC at the nominal bubbling rate of 9 lpm and also with optimized bubbling to achieve maximum production rates; these conditions were selected to allow comparison to results obtained previously with other HLW simulants [16, 17, 20-22, 27, 32]. The feeds with MnO were processed as the feed rate was adjusted to provide the desired complete cold cap. Glass production rates of 920 and 1560 kg/m 2 /day were achieved with nominal and optimized P P bubbling, respectively. The rate obtained at nominal conditions was less than that achieved for any of the other high waste loading formulations and marginally above the WTP HLW baseline requirement; however, processing rates can exceed the WTP HLW baseline requirement by a factor of two with optimization of melt pool bubbling. Additional DM100 melter tests were conducted with feeds containing two other forms of manganese (MnO2 and MnCO3) under nominal conditions (1150°C glass temperature, 9 lpm bubbling) so that the effect of the form of manganese on feed processing rate and processing characteristics could be determined. Production rates for these feeds were at or below the WTP HLW baseline requirement of 800 kg/m2/day and showed the following melt rate trend: MnO2 < MnCO3 < MnO This trend is contrary to that observed for feeds with different forms of iron, which showed no effect on production rate with transition metal oxidation state [29]. Also, the relative percentage change in production rate with different forms of manganese is twice that for different forms of iron, despite the manganese content in the HLW-HMn-20 glass composition being less than a third of the iron concentration in the HLW-NG-Fe2 glass composition. Feeds with MnO2 subjected to VGF testing were also shown to be slower melting than feeds with other forms of manganese. 37 Samples of the glass product were collected and analyzed for composition, crystalline phases, iron oxidation state, and product quality from each test. Crystalline phases in the form of spinels were measured in melter glasses at 0.6 to 1.1 volume percent with no clear differences based on the form of manganese in the feed. The measured amount of spinels in melter glasses was higher than the 0.5 volume percent measured on crucible melt glasses. The measured iron oxidation state of melter glasses ranged from totally oxidized in tests with MnO and MnO2 to about four and half percent divalent iron in tests with MnCO3. The small amounts of divalent iron in tests with MnCO3 are probably attributable to trace contamination of the MnCO3 with organic carbon. Glass from each of the tests far exceeded chemical durability criteria for the PCT and TCLP methods. Particulate emissions while processing the HLW-HMn-20 glass composition constituted only 0.23 to 0.34 percent of feed solids and were lower than for most HLW compositions tested previously. Carryover values for comparable tests conducted with MnO, MnO2, and MnCO3 ranged from only 0.23 to 0.3 percent of feed solids with no obvious trends between tests with different forms of manganese. The composition of the particulate in the melter exhaust is reflective of the feed composition with some enrichment (boron, chromium, alkalis, lead, fluorine, thallium, and sulfur) or depletion (silicon, nickel, phosphorus, and zirconium) based on elemental volatility. No difference in these trends was observed with the changing form of manganese over the course of the tests, indicating that the relative carryover of manganese is not affected by the mineralogy or grain size of the different forms of manganese. The composition of the particulate was confirmed by retrieval and analysis of solids from the cyclone filter in the off-gas system. XRD analysis of these particulates indicates entrainment of feed minerals in the exhaust as well as enrichments of the most volatile elements, particularly thallium and sulfur. Manganese was observed as either MnO or MnO2 in cyclone deposits from the respective tests, while MnCO3 was not detected in any of the cyclone deposits indicating that MnCO3 more readily decomposes in the cold cap. The results of the testing presented herein further demonstrate the viability of the enhancement and optimization strategies that have been developed in previous work for ORP [3, 16, 17, 21-22, 27-29, 32, 33, 54]. The results extend the potential for enormous savings in cost and schedule that result from that work. It is recommended that testing and evaluation of these very successful strategies be continued in order to provide a solid basis for their broad implementation in order to maximize the cost and schedule benefits while minimizing technical risk. Specifically, a glass formulation for a high manganese HLW stream was developed which conforms to all product quality and processing requirements. The waste loading of 35 wt% was limited by spinel formation since the waste stream also contained relatively high concentrations of nickel and chromium, which also contribute to spinel crystallization. Production rates exceeding the WTP HLW baseline were obtained for feed containing MnO but not with MnO2 or MnCO3 at nominal conditions. These observations further confirm that the form of waste components can significantly affect glass production rates [3, 16, 27-29] and, in the case of manganese, at concentrations of less than five weight percent oxide. The extent of secondary phase formation, amount of reduced iron, and product quality were unaffected by the form of manganese in the melter feed. The forms of manganese in the deposits within the off-gas system were the same as that in the feed, indicating entrainment carry over from the cold cap. 38 These results show the importance of evaluating the effects of all probable forms of waste components on the vitrification process. While identifying the forms of waste components is complicated by limited knowledge and sampling of tank wastes, as well as chemical reactions occurring in tanks over time, during pretreatment, and in the melter feed, the available information can be used to perform testing to assess the potential magnitude of these effects and to develop useful bounds. The results from the present work indicate that the Batch 3939 high-manganese HLW stream would benefit from additional formulation development to further increase the potential processing rate for all forms of manganese likely to be present. Testing is also recommended to address other forms of manganese likely to be present in Hanford HLW streams. 39 SECTION 7.0 REFERENCES [1] “HLW Glass Development Testing,” Contract Number DE- RP27-07RV14884, US Department of Energy, Office of River Protection, Richland, WA, 2007. [2] “Test and Evaluate High Level Waste (HLW) Vitrification System Improvements,” Contract Number DE-AC27-06RV14790, US Department of Energy, Office of River Protection, Richland, WA, April, 2006. [3] “High Level Waste Vitrification System Improvements,” K.S. Matlack, H. Gan, W. Gong, I.L. Pegg, C.C. Chapman, and I. Joseph, Final Report, VSL-07R1010-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 04/16/07. [4] “Glass Formulation and Testing with RPP-WTP HLW Simulants,” W.K. Kot, and I.L. Pegg, Final Report, VSL-01R2540-2, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 2/16/01. [5] “Glass Formulation to Support Melter Runs with HLW Simulants,” W.K. Kot, K. Klatt, and I.L. Pegg, Final Report, VSL-03R3760-2, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 09/30/03. [6] “HLW Glass Formulation to Support C-106/AY-102 Actual Waste Testing,” W.K. Kot and I.L. Pegg, Final Report, VSL-04R4770-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 08/12/04. [7] “Development of Phase 1 IHLW Models for PCT Response and One-Percent Crystal Fraction Temperature (T1%),” W.K. Kot, H. Gan, Z. Feng, F. Perez-Cardenas, I.L. Pegg, S.K. Cooley, and G.F. Piepel, Final Report, VSL-05R5780-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 04/12/05. [8] “Preparation and Testing (T1% and PCT) of HLW Matrix Glasses to Support WTP Property-Composition Model Development,” W.K. Kot, H. Gan, and I.L. Pegg, Final Report, VSL-05R5780-2, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 10/12/05. [9] “Summary and Recommendations on Viscosity and Conductivity Model Forms to Support HLW Vitrification,” H. Gan, Z. Feng, and I.L. Pegg, Letter Report, VSL-04L4780-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 09/08/04. 40 [10] “Integrated DM1200 Melter Testing of Bubbler Configurations Using HLW AZ-101 Simulants,” K.S. Matlack, W. Gong, T. Bardakci, N. D’Angelo, W. Lutze, R.A. Callow, M. Brandys, W.K. Kot, and I.L. Pegg, Final Report, VSL-04R4800-4, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 10/05/04. [11] “Melter Tests with AZ-101 HLW Simulant Using a DuraMelter 100 Vitrification System,” K.S. Matlack, W.K. Kot, and I.L. Pegg, Final Report, VSL-01R10N0-1, Rev. 1, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 02/25/01. [12] “DuraMelter 100 HLW Simulant Validation Tests with C-106/AY-102 Feeds,” K.S. Matlack, W. Gong and I.L. Pegg, Final Report, VSL-05R5710-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 6/2/05. [13] “Integrated DM1200 Melter Testing of HLW C-106/AY-102 Composition Using Bubblers,” K.S. Matlack, W. Gong, T. Bardakci, N. D’Angelo, W. Kot and I.L. Pegg, Final Report, VSL-03R3800-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 9/15/03. [14] “Integrated DM1200 Melter Testing of HLW C-104/AY-101 Compositions Using Bubblers,” K.S. Matlack, W. Gong, T. Bardakci, N. D’Angelo, W. Kot and I.L. Pegg, Final Report, VSL-03R3800-3, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 11/24/03. [15] “Integrated DM1200 Melter Testing Using AZ-102 and C-106/AY-102 HLW Simulants: HLW Simulant Verification,” K.S. Matlack, W. Gong, T. Bardakci, N. D’Angelo, M. Brandys, W.K. Kot, and I.L. Pegg, Final Report, VSL-05R5800-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 6/27/05. [16] “Melter Throughput Enhancements for High Iron HLW,” K.S. Matlack, H. Gan, M. Chaudhuri, W.K. Kot, I.L. Pegg and I. Joseph Final Report, VSL-12R2490-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 5/31/12. [17] “Melter Testing of New High-Bismuth HLW Formulations,” K.S. Matlack, W.K. Kot, H. Gan, I.L. Pegg, and I. Joseph, Final Report, VSL-13R2770-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 3/25/13. [18] “Management of High Sulfur HLW,” K.S. Matlack, W.K. Kot, I.L. Pegg, and I. Joseph, Final Report, VSL-13R2920-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 10/31/13. [19] “Enhanced Sulfate Management in HLW Glass Formulations,” K.S. Matlack, W.K. Kot, H. Gan, I.L. Pegg, and I. Joseph, Final Report, VSL-12R2540-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 9/21/12. 41 [20] “High Waste Loading Glass Formulation Development for High-Cr HLW,” K.S. Matlack, H. Gan, M. Chaudhuri, W.K. Kot, and I.L. Pegg, Final Report, VSL-14R3060- 1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 4/28/14. [21] “High Waste Loading Glass Formulation Development for High-Sr HLW,” K.S. Matlack, H. Gan, M. Chaudhuri, W.K. Kot, I.L. Pegg, and I. Joseph, Final Report, VSL-14R3260- 1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 2/4/15. [22] “High Waste Loading Glass Formulation Development for High-Zr HLW,” K.S. Matlack, W.K. Kot, I.L. Pegg, and I. Joseph, Final Report, VSL-15R3250-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 2/23/15. [23] “Effects of High Spinel and Chromium Oxide Crystal Contents on Simulated HLW Vitrification in DM100 Melter Tests,” K.S. Matlack, W.K. Kot, W. Gong, W. Lutze, I. Joseph, and I.L. Pegg, Final Report, VSL-09R1520-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 6/19/09. [24] “Hanford Waste Physical and Rheological Properties: Data and Gaps,” B.E. Wells, J.L. Huckaby, J.M. Tingey, D.E. Kurath, S.K. Cooley, R.C. Daniel, L.A. Mahoney, C.A. Burns, K.K. Anderson, Y. Onishi, and E.C. Buck, PNNL-20646, EMSP-RPT-006, August 2011. [25] “Advances in Geochemical Testing of Key Contaminants in Residual Hanford Tank Waste,” W.J. Deutsch, H.T. Schaef, K.M. Krupka, S.M. Heald, K.J. Cantrell, B.W. Arey, C.F. Brown, R.K. Kukkadapu, PNNL-15372, November 2005. [26] “Hanford Waste Mineralogy Reference Report,” S.J. Harrington, Washington River Protection Solutions, LLC, RPP-RPT-46618, Rev 2, June 2011. [27] “Melt Rate Enhancement for High Aluminum HLW Glass Formulations,” K.S. Matlack, H. Gan, M. Chaudhuri, W.K. Kot, W. Gong, T. Bardakci, and I.L. Pegg, Final Report, VSL-08R1360-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 12/19/08. [28] “DM100 and DM1200 Melter Testing with High Waste Loading Glass Formulations for Hanford High-Aluminum HLW Streams,” K.S. Matlack, H. Gan, M. Chaudhuri, W.K Kot, W. Gong, T. Bardakci, I. Joseph, and I.L. Pegg, Final Report, VSL-10R1690-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 8/16/10. [29] “Effect of the Form of Iron on HLW Melt Rate,” K.S. Matlack, C. Viragh, W.K. Kot, I.L. Pegg, and I. Joseph, Final Report, VSL-15R3430-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 4/27/15. 42 [30] "Effect of Feed Melting, Temperature History, and Minor Component Addition on Spinel Crystallization in High-Level Waste Glass," P. Izak, P. Hrma, B.W. Arey, and T.J. Plaisted, J. Non-Cryst. Solids, 289, 17 (2001). [31] “Hanford Tank Waste Operations Simulation (HTWOS) Version 6.6.1 Model Design Document,” Rev. 6, Washington River Protection Solutions, LLC, Richland, WA, 2011. [32] “High Waste Loading Glass Formulation Development for High-P HLW,” K.S. Matlack, W.K. Kot, and I.L. Pegg, Final Report, VSL-17R3700-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 5/9/17. [33] “Tests with High-Bismuth HLW Glasses,” K.S. Matlack, H. Gan, W.K. Kot, M. Chaudhuri, R.K. Mohr, D. A. McKeown, T. Bardakci, W. Gong, A. C. Buechele, and I.L. Pegg, Final Report, VSL-10R1780-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 12/13/10. [34] “High Waste Loading Glass Formulation Development for High-Mn HLW,” K.S. Matlack, W.K. Kot, and I.L. Pegg, Test Plan, VSL-15T3810-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 2/8/16. [35] “Quality Assurance Project Plan for ORP/ RPP-WTP Support Activities Conducted by VSL,” Vitreous State Laboratory, QAPP-ORP, Rev. 6, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 9/14/16. [36] “Master List of Controlled VSL Manuals and Standard Operating Procedures in Use,” QA-MLCP, Rev. 151, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 3/20/17. [37] “Standard Test Methods for Determining Chemical Durability of Nuclear, Hazardous, and Mixed Waste Glasses and Multiphase Glass Ceramics: The Product Consistency Test (PCT),” ASTM C1285-02, American Society for Testing and Materials, West Conshohocken, PA, 2008. [38] “Round Robin Testing of a Reference Glass for Low-Activity Waste Forms,” W.L. Ebert and S.F. Wolf, Department of Energy report ANL-99/22, Argonne National Laboratory, Argonne, IL, 1999. [39] “Characterization of the Defense Waste Processing Facility (DWPF) Environmental Assessment (EA) Glass Standard Reference Material,” C.M. Jantzen, N.E. Bibler, D.C. Beam, C.L. Crawford, and M.A. Pickett, WSRC-TR-92-346, Westinghouse Savannah River Company, Aiken, SC, June, 1993. [40] “River Protection Project System Plan,” ORP-11242, Revision 6, U.S. Department of Energy, Office of River Protection, Richland, WA, October 2011. 43 [41] “Estimate of Hanford Waste Insoluble Solid Particle Size and Density Distribution,” B.E. Wells, M.A. Knight, E.C. Buck, S.K. Cooley, R.C. Daniel, L.A. Mahoney, P.A. Meyer, A.P. Poloski, J.M. Tingey, W.S. Callaway III, G.A. Cooke, M.E. Johnson, M.G. Thien, D.J. Washenfelder, J.J. Davis, M.N. Hall, G.L. Smith, S.L. Thomson, and Y. Onishi., PNWD-3824 (WTP-RPT-153, Rev. 0), Battelle-Pacific Northwest Division, Richland, Washington, 2007. [42] “Small Scale Melter Testing of HLW Algorithm Glasses: Matrix 2 Tests,” K.S. Matlack, W.K. Kot, W. Gong and I.L. Pegg, Final Report, VSL-08R1220-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, June 27, 2008. [43] “Small Scale Melter Testing of HLW Algorithm Glasses: Matrix 1 Tests,” K.S. Matlack, W.K. Kot, W. Gong and I.L. Pegg, Final Report, VSL-07R1220-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, November 12, 2007. [44] “X-Ray Absorption Studies of Manganese Valence and Local Environment in Borosilicate Waste Glasses,” D.A. McKeown, W.K. Kot, and I.L. Pegg, J. Non-Cryst. Solids, Vol. 328, 71-89 (2003). [45] “Support for HLW Direct Feed,” K.S. Matlack, W.K. Kot, I.S. Muller, I.L. Pegg, and I. Joseph, Final Report, VSL-14R3090-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, June 26, 2014. [46] “Support for HLW Direct Feed – Phase 2,” W.K. Kot, K.S. Matlack, I.L. Pegg, and I. Joseph, Final Report, VSL-15R3440-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, September 28, 2015. [47] “Design, Construction, and Commissioning of the Hanford Tank Waste Treatment and Immobilization Plant,” Contract Number: DE-AC27-01RV14136, U.S. Department of Energy, Office of River Protection, 2000 (as amended). [48] “River Protection ProjectWaste Treatment Plant Engineering Specification for High Level Waste Melters,” R.P. Casassa, BNI Specification, 24590-HLW-3PS-AE00-TP001, Rev. 0, River Protection Project, Waste Treatment Plant, Richland, WA, 1/31/05. [49] “Enhanced K-3 Refractory Corrosion with LAW AZ-102 Glass Formulations,” I.S. Muller, H. Gan, A.C. Buechele, and I L. Pegg, Summary Report, VSL-02S4600-1 Rev. 0, Vitreous State Laboratory, Washington, DC, 6/25/02. [50] “Waste Loading Enhancements for Hanford LAW Glasses,” I.S. Muller, K.S. Matlack, H. Gan, I. Joseph, and I.L. Pegg, Final Report, VSL-10R1790-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 12/1/10. 44 [51] “Glass Formulation Development for Al, Fe, and Na Phosphate HLW,” K.S. Matlack, W.K. Kot, and I.L. Pegg, Test Plan, VSL-15T3820-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 2/16/16. [52] “Petition to Delist Immobilized High-Level Waste Generated at the Waste Treatment and Immobilization Plant,” D.B. Blumenkranz, DOE/ORP-2006-03, Rev. 0, U.S. Department of Energy, Office of River Protection, Richland, WA, 2006. [53] “Data Quality Objectives Process in Support of LDR/Delisting at the WTP,” J. Cook and D.B. Blumenkranz, 24590-WTP-RPT-ENV-01-012, Rev. 2, River Protection Project, Waste Treatment Plant, Richland, WA, 3/26/03. [54] “Effect of Form of Chromium on Spinel Formation,” K.S. Matlack, H. Gan, M. Chaudhuri, W.K. Kot, I.L. Pegg, and I. Joseph, Final Report, VSL-16R3540-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, June 30, 2016. [55] “Technetium/Cesium Volatility in DM100 Tests Using HLW AZ-102 and LAW Sub-Envelope A1 Simulants,” K.S. Matlack, W.K. Kot, and I.L. Pegg, Final Report, VSL-04R4710-1, Rev. 0, Vitreous State Laboratory, The Catholic University of America, Washington, DC, 9/28/04. 45 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 1.1. Ranking Basis for Feed Conversion after 30 Minute VGF Test. 1 Very Fast, all feed converted 2 Fast with minor residue on side wall 3 Moderate with foamy residue on side wall 4 Slow with thick foam layer 5 Slow with partially collapsed dome 6 Very slow with fully developed dome T-1 HFO-73169, Rev. 0 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.1. Calcined Composition (wt%) of High-Manganese HLW Simulant. HLW Composition from Normalized HLW Oxide HTWOS Model Run Simulant Composition (Waste Batch 3939)(1) Al2O3 29.70% 31.093% B 2O 3 0.29% 0.304% Bi2O3 4.14% 4.334% CaO 1.40% 1.466% Cr2O3 2.43% 2.544% F 0.24% 0.251% Fe2O3 8.95% 9.370% K 2O 0.60% 0.628% La2O3 0.63% 0.660% MgO 0.38% 0.398% MnO 13.70% 14.343% Na2O 19.78% 20.708% Nd2O3 0.13% 0.136% NiO 1.83% 1.916% P2O5 2.84% 2.973% PbO 0.43% 0.450% SO3 0.94% 0.984% SiO2 6.28% 6.575% SrO 0.31% 0.325% Tl2O 0.17% 0.178% UO3 3.59% omitted WO3 0.11% 0.115% ZrO2 0.24% 0.251% TOTAL 99.11% 100.00% (1) Minor oxides (i.e., < 0.1 wt%) omitted. T-2 HFO-73169, Rev. 0 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.2. Composition of High-Manganese HLW Simulant to Produce 100 kg of Waste Oxides (21.50 wt% total solids). Starting Material Target Weight (kg)(1) Al(OH)3 48.053 H3BO3 0.545 Bi2O3 4.378 CaCO3 2.642 Cr2O3 2.570 NaF 0.561 Fe(OH)3 (13% slurry) 96.452 K2CO3 0.931 La2O3 0.666 MgO 0.402 MnO(2) 14.487 NaOH 16.512 Nd2O3 0.137 Ni(OH)2 2.402 Na3PO4 6.937 PbO 0.455 Na2SO4 1.764 SiO2 6.641 SrCO3 0.474 Tl2O 0.180 WO3 0.116 Zr(OH)4·xH2O (x = 4 to 5) 0.509 Na2CO3 4.450 NaNO2 0.018 NaNO3 1.085 H2C2O4·2H2O 0.139 Water 389.253 TOTAL 602.759 (1) Target weights adjusted for projected assay values of starting materials. (2) MnO will be replaced with either MnO 2 or MnCO3 on a Mn basis for specific tests. T-3 HFO-73169, Rev. 0 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.3. Target and XRF Analyzed Compositions of HLW-HMn Glasses. - Waste HLW-HMn-1 HLW-HMn-2 HLW-HMn-3 HLW-HMn-4 HLW-HMn-5 HLW-HMn-6 HLW-HMn-7 Waste Loading 100 40 45 40 45 40 45 40 (wt%) Formulation HLW M-K, M-Li, M-K, M-Li, M-Na M-Li, M-Na H-Li, M-Na VH-Li VH-Na H-K, M-Na Key Waste M-Na Data Type Target Target XRF Target XRF Target XRF Target XRF Target XRF Target XRF Target XRF Al2O3 31.09 12.44 12.12 13.99 13.78 12.44 12.28 13.99 13.73 12.44 12.21 13.99 13.61 12.44 12.26 B2O3* 0.30 17.12 17.12 17.14 17.14 18.12 18.12 17.14 17.14 15.12 15.12 14.14 14.14 18.12 18.12 Bi2O3 4.33 1.73 1.72 1.95 1.95 1.73 1.74 1.95 1.96 1.73 1.78 1.95 2.06 1.73 1.70 CaO 1.47 0.59 0.62 0.66 0.68 0.59 0.61 0.66 0.70 0.59 0.63 0.66 0.76 0.59 0.63 Cr2O3 2.54 1.02 0.93 1.14 1.06 1.02 0.88 1.14 0.99 1.02 0.92 1.14 1.06 1.02 0.93 F 0.25 0.10 NA 0.11 NA 0.10 NA 0.11 NA 0.10 NA 0.11 NA 0.10 NA Fe2O3 9.37 3.75 3.68 4.22 4.14 3.75 3.71 4.22 4.10 3.75 3.68 4.22 4.27 3.75 3.60 K2O 0.63 3.25 3.19 0.28 0.31 0.25 0.28 2.28 2.22 0.25 0.28 0.28 0.34 5.25 5.23 La2O3 0.66 0.26 0.23 0.30 0.22 0.26 0.21 0.30 0.23 0.26 0.17 0.30 0.22 0.26 0.19 Li2O* 0.00 2.00 2.00 2.00 2.00 4.00 4.00 2.00 2.00 6.00 6.00 0.00 0.00 0.00 0.00 MgO 0.40 0.16 0.14 0.18 0.21 0.16 0.15 0.18 0.20 0.16 0.18 0.18 0.16 0.16 0.15 MnO 14.34 5.74 5.66 6.45 6.35 5.74 5.70 6.45 6.40 5.74 5.79 6.45 6.58 5.74 5.60 Na2O 20.71 10.28 10.31 11.32 11.42 10.28 10.29 11.32 11.61 8.28 8.14 18.32 18.10 10.28 10.24 Nd2O3 0.14 0.05 0.04 0.06 0.04 0.05 0.05 0.06 0.05 0.05 0.06 0.06 0.05 0.05 0.06 NiO 1.92 0.77 0.86 0.86 0.92 0.77 0.84 0.86 0.89 0.77 0.83 0.86 0.98 0.77 0.83 P2O5 2.97 1.19 1.25 1.34 1.37 1.19 1.23 1.34 1.41 1.19 1.22 1.34 1.44 1.19 1.27 PbO 0.45 0.18 0.18 0.20 0.21 0.18 0.18 0.20 0.20 0.18 0.19 0.20 0.23 0.18 0.17 SiO2 6.57 38.63 39.24 36.96 37.46 38.63 39.01 34.96 35.40 41.63 42.06 34.96 35.17 37.63 38.35 SrO 0.32 0.13 0.11 0.15 0.12 0.13 0.11 0.15 0.12 0.13 0.11 0.15 0.13 0.13 0.11 TiO2 0.00 0.00 0.01 0.00 0.02 0.00 0.01 0.00 0.02 0.00 0.02 0.00 0.01 0.00 0.02 Tl2O 0.18 0.07 0.07 0.08 0.08 0.07 0.07 0.08 0.08 0.07 0.07 0.08 0.08 0.07 0.07 SO3 0.98 0.39 0.34 0.44 0.36 0.39 0.36 0.44 0.37 0.39 0.38 0.44 0.43 0.39 0.33 V2O5 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 WO3 0.11 0.05 0.05 0.05 0.08 0.05 0.07 0.05 0.07 0.05 0.06 0.05 0.05 0.05 0.04 ZrO2 0.25 0.10 0.11 0.11 0.11 0.10 0.10 0.11 0.12 0.10 0.11 0.11 0.12 0.10 0.10 Sum 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 NA: Not Analyzed *: Target values used with XRF data Formulation Key:VH=Very High; H=High; M=Medium; Letters after dash indicate component T-4 HFO-73169, Rev. 0 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.3. Target and XRF Analyzed Compositions of HLW-HMn Glasses (continued). HLW-HMn-8 HLW-HMn-9 HLW-HMn-10 HLW-HMn-11 HLW-HMn-12 HLW-HMn-13 HLW-HMn-14 Waste Loading 45 35 35 35 35 35 35 (wt%) Formulation Key H-Ca, H-Na VH-Li VH-K, M-Li VH-K VH-K, H-B VH-K, M-Li, M-V VH-K, M-Li, M-P Data Type Target XRF Target XRF Target XRF Target XRF Target XRF Target XRF Target XRF Al2O3 13.99 13.69 10.88 10.79 10.88 7.50 10.88 10.83 10.88 10.77 10.88 10.49 10.88 10.54 B2O3* 17.14 17.14 17.11 17.11 18.11 18.11 18.11 18.11 19.11 19.11 18.11 18.11 18.11 18.11 Bi2O3 1.95 2.01 1.52 1.53 1.52 1.56 1.52 1.49 1.52 1.44 1.52 1.58 1.52 1.51 CaO 4.66 4.90 0.51 0.54 0.51 0.58 0.51 0.54 0.51 0.50 0.51 0.56 0.51 0.52 Cr2O3 1.14 1.09 0.89 0.86 0.89 0.87 0.89 0.79 0.89 0.76 0.89 0.97 0.89 0.84 F 0.11 NA 0.09 NA 0.09 NA 0.09 NA 0.09 NA 0.09 NA 0.09 NA Fe2O3 4.22 4.22 3.28 3.27 3.28 3.33 3.28 3.09 3.28 3.00 3.28 3.23 3.28 3.19 K2O 0.28 0.30 0.22 0.25 8.22 8.18 10.22 9.64 8.22 7.87 8.22 7.99 8.22 7.91 La2O3 0.30 0.22 0.23 0.13 0.23 0.17 0.23 0.17 0.23 0.17 0.23 0.16 0.23 0.17 Li2O* 0.00 0.00 6.00 6.00 2.00 2.00 0.00 0.00 0.00 0.00 2.00 2.00 2.00 2.00 MgO 0.18 0.15 0.14 0.15 0.14 0.15 0.14 0.16 0.14 0.13 0.14 0.16 0.14 0.17 MnO 6.45 6.42 5.02 4.88 5.02 5.00 5.02 4.82 5.02 4.87 5.02 4.93 5.02 4.82 Na2O 12.32 12.21 7.25 7.15 7.25 7.79 7.25 7.57 7.25 8.10 7.25 7.26 7.25 7.04 Nd2O3 0.06 0.05 0.05 0.05 0.05 0.05 0.05 0.08 0.05 0.04 0.05 0.05 0.05 0.05 NiO 0.86 0.94 0.67 0.75 0.67 0.74 0.67 0.70 0.67 0.67 0.67 0.73 0.67 0.77 P2O5 1.34 1.40 1.04 1.11 1.04 1.14 1.04 1.10 1.04 1.11 1.04 1.09 3.04 3.16 PbO 0.20 0.22 0.16 0.16 0.16 0.16 0.16 0.16 0.16 0.16 0.16 0.16 0.16 0.16 SiO2 33.96 34.22 44.30 44.66 39.30 42.02 39.30 40.24 40.30 40.70 36.30 36.86 37.30 38.41 SrO 0.15 0.12 0.11 0.09 0.11 0.09 0.11 0.08 0.11 0.08 0.11 0.08 0.11 0.08 TiO2 0.00 0.02 0.00 0.02 0.00 0.02 0.00 0.01 0.00 0.02 0.00 0.04 0.00 0.04 Tl2O 0.08 0.09 0.06 0.06 0.06 0.06 0.06 0.05 0.06 0.06 0.06 0.06 0.06 0.06 SO3 0.44 0.39 0.34 0.28 0.34 0.32 0.34 0.26 0.34 0.30 0.34 0.29 0.34 0.30 V2O5 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 3.00 3.07 0.00 0.00 WO3 0.05 0.06 0.04 0.05 0.04 0.06 0.04 0.03 0.04 0.06 0.04 0.04 0.04 0.05 ZrO2 0.11 0.12 0.09 0.09 0.09 0.10 0.09 0.09 0.09 0.08 0.09 0.09 0.09 0.09 Sum 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 NA: Not Analyzed *: Target values used with XRF data Formulation Key:VH=Very High; H=High; M=Medium; Letters after dash indicate component T-5 HFO-73169, Rev. 0 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.3. Target and XRF Analyzed Compositions of HLW-HMn Glasses (continued). HLW-HMn-15 HLW-HMn-16 HLW-HMn-17 HLW-HMn-18 HLW-HMn-19 HLW-HMn-20 Waste Loading 32 32 35 35 35 35 (wt%) Formulation Key VH-Li VH-K, M-Li VH-K, M-Li, Zr VH-K, M-Li, Zr/Al from HLW07-20 M-K, H-Li, Zr Data Type Target XRF Target XRF Target XRF Target XRF Target XRF Target XRF Al2O3 9.95 9.41 9.95 9.72 10.88 10.34 13.88 13.40 10.88 10.34 10.88 10.35 B2O3* 18.10 18.10 18.10 18.10 17.11 17.11 17.11 17.11 15.11 15.11 16.11 16.11 Bi2O3 1.39 1.53 1.39 1.37 1.52 1.57 1.52 1.53 1.52 1.56 1.52 1.56 CaO 0.47 0.49 0.47 0.45 0.51 0.53 0.51 0.56 0.51 0.54 0.51 0.55 Cr2O3 0.81 0.79 0.81 0.74 0.89 0.83 0.89 0.79 0.89 0.82 0.89 0.78 F 0.08 NA 0.08 NA 0.09 NA 0.09 NA 0.09 NA 0.09 NA Fe2O3 3.00 3.14 3.00 2.95 3.28 3.29 3.28 3.25 3.28 3.34 3.28 3.24 K2O 0.20 0.21 8.20 7.71 8.22 8.05 8.22 7.98 0.22 0.24 4.22 4.09 La2O3 0.21 0.11 0.21 0.15 0.23 0.16 0.23 0.12 0.23 0.18 0.23 0.16 Li2O* 7.00 7.00 3.00 3.00 2.00 2.00 2.00 2.00 4.00 4.00 3.50 3.50 MgO 0.13 0.15 0.13 0.14 0.14 0.15 0.14 0.15 0.14 0.15 0.14 0.18 MnO 4.59 4.63 4.59 4.45 5.02 5.10 5.02 5.00 5.02 5.05 5.02 4.98 Na2O 6.63 6.31 6.63 6.68 7.25 6.83 7.25 7.06 8.25 8.00 7.25 7.19 Nd2O3 0.04 0.06 0.04 0.05 0.05 0.06 0.05 0.03 0.05 0.05 0.05 0.05 NiO 0.61 0.72 0.61 0.68 0.67 0.76 0.67 0.74 0.67 0.76 0.67 0.71 P2O5 0.95 0.99 0.95 1.00 1.04 1.07 1.04 1.10 1.04 1.02 1.04 1.06 PbO 0.14 0.15 0.14 0.15 0.16 0.17 0.16 0.16 0.16 0.15 0.16 0.16 SiO2 45.10 45.65 41.10 42.07 37.30 38.45 35.30 36.38 45.30 46.08 40.80 41.81 SrO 0.10 0.09 0.10 0.08 0.11 0.08 0.11 0.08 0.11 0.08 0.11 0.08 TiO2 0.00 0.04 0.00 0.03 0.00 0.04 0.00 0.05 0.00 0.04 0.00 0.04 Tl2O 0.06 0.07 0.06 0.06 0.06 0.05 0.06 0.06 0.06 0.07 0.06 0.06 SO3 0.31 0.27 0.31 0.31 0.34 0.23 0.34 0.31 0.34 0.29 0.34 0.27 V2O5 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.00 WO3 0.04 0.04 0.04 0.04 0.04 0.03 0.04 0.04 0.04 0.04 0.04 0.04 ZrO2 0.08 0.07 0.08 0.06 3.09 3.06 2.09 2.04 2.09 2.08 3.09 2.98 Sum 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 99.9 NA: Not Analyzed *: Target values used with XRF data Formulation Key:VH=Very High; H=High; M=Medium; Letters after dash indicate component T-6 HFO-73169, Rev. 0 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.4. Summary of Characterization Results for HLW-HMn Glasses. HLW- HLW- HLW- HLW- HLW- HLW- HLW- HLW- HLW- HLW- Glass ID HMn-1 HMn-2 HMn-3 HMn-4 HMn-5 HMn-6 HMn-7 HMn-8 HMn-9 HMn-10 Formulation Waste Loading 40 45 40 45 40 45 40 45 35 35 (wt%) Formulation M-K, M- M-Li, M- H-Li, M- M-K, M- H-K, M- H-Ca, H- VH-K, M- VH-Li VH-Na VH-Li Key** Li, M-Na Na Na Li, M-Na Na Na Li Glass as Melted 1.6 3 2 4.9 0.9 3 3.1 3.4 0.8 0.5 (wt% by XRD*) Sp: Sp: Sp: 1%, Sp: 0.7%, 950oC (Vol% Sp: Sp: Sp: 2.40%, Sp: Sp: 2.47%, Sp: 2% Cr2O3: Cr2O3: by SEM) 1.66% 2.22% 1.33% Cr2O3: 1.21% 2.37% CaP: trace trace trace 1.45% Sp: Sp: Sp: 1%, 900oC (Vol% Sp: Sp: Sp: Sp: Sp: 2.64%, 0.94%, Sp: 1.7% Sp: 2.3% Cr2O3: by SEM) 1.48% 2.41% 2.65% 1.75% 2.69% CaP: Cr2O3: Crystallization trace 1.78% trace Sp: 2.68%, Sp: 2.8%, Sp: 1.25, 850oC (Vol% Sp: Sp: Sp: Sp: Sp: Sp: CaP: 1- NaCaP: Sp: 1.3% Cr2O3: by SEM) 1.96% 2.76% 2.08% 3.04% 2.08% 3.13% 2%, trace trace Cr2O3: 1- 2% Sp: Sp: 3.13%, Sp: 800oC (Vol% Sp: Sp: Sp: Sp: 2.59%, Sp: NaCaP<0 3.22%, Sp: 1.7% Sp: 1.5% by SEM) 2.25% 3.37% 2.25% 3.34% LiP: 3.35% .2%, CaP: 2- trace CaP<0.1 3% % CCC (Vol% - - - - - - - - - Sp: 1.8% by SEM) Viscosity Processing (Poise at - - - - - - - - 32 34 Property 1150oC) Conductivity (S/cm at - - - - - - - - 0.34 0.17 1150oC) Quenched PCT - - - - - - - - 1.553 10.368 Resistance B (g/L) Leaching CCC PCTB - - - - - - - - 1.87 9.827 (g/L) TCLP - - - - - - - - PASS PASS (Pass/Fail) *: Estimated from XRD powder pattern analysis without an internal standard **: "VH": Very High, "H": High, "M": Medium; Letters after dash indicate component Sp: Spinel; LiP: Lithium phosphate; CaP: Calcium phosphate; NaCaP: Sodium calcium phosphate - Empty data field T-7 HFO-73169, Rev. 0 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.4. Summary of Characterization Results for HLW-HMn Glasses (continued). HLW- HLW- HLW- HLW- HLW- HLW- HLW- HLW- HLW- HLW- Glass ID HMn-11 HMn-12 HMn-13 HMn-14 HMn-15 HMn-16 HMn-17 HMn-18 HMn-19 HMn-20 Formulation Waste Loading 35 35 35 35 32 32 35 35 35 35 (wt%) Formulation VH-K, H- VH-K, M- VH-K, M- VH-K, M- VH-K, M- VH-K, M- H-Si, H- M-K, H- VH-K VH-Li Key** B Li, M-V Li, M-P Li Li, Zr Li, Zr/Al Li, Zr Li, Zr Glass as melted (wt%, 1.5 1.8 0.9 1.3 0.3 1.0 1.4 1.9 1.6 1 by XRD*) Sp: Sp: Sp: Sp: Sp: 1.4%, Sp: 1.6%, Sp: 1.1%, 950oC (Vol% 0.98%, 0.86%, 1.09%, 0.78%, Cr2O3: Cr2O3: Cr2O3: Sp: 0.70% Sp: 0.65% SP: 0.88% by SEM) Cr2O3: Cr2O3: Cr2O3: Cr2O3: trace trace trace trace trace trace trace Sp: Sp: Sp: Sp: Sp: Sp: 1.8%, Sp: 1.9%, Sp: 1.4%, 900oC (Vol% 0.87%; 1.09%, 1.57%, 1.22%; 1.03%; Cr2O3: Cr2O3: Sp: 1.3% Cr2O3: Sp: 0.68% by SEM) Cr2O3: Cr2O3: Cr2O3: Cr2O3: Cr2O3: Crystallization trace trace trace trace trace trace trace trace Sp: Sp: Sp: Sp: 2%, Sp: 2.1%, Sp: 1.6%, Sp: 1.5%; 850oC (Vol% Sp: 0.9%; 1.34%, 1.81%, 1.52%; Cr2O3: CaP/Cr2O Sp: 1.8% Cr2O3: Sp: 1.03% Cr2O3: by SEM) Cr2O3: trace Cr2O3: Cr2O3: Cr2O3: trace 3: trace trace trace trace trace trace Sp: 2.3%, Sp: Sp: Sp: Sp: 2.2%, Sp: 2.3%, Sp: 2.0%, Sp: 1.12%; 800oC (Vol% CaP:0.1% 2.17%, 1.68%; 1.66%; NaCaP:0. Cr2O3: NaCaP:0. Void: trace Sp: 1.2% Sp: 1.77% by SEM) , Cr2O3: Cr2O3: Cr2O3: Cr2O3: 2% 0.1% 1% phosphate? trace trace trace trace Sp: 1.9%, Sp: 2.1%, NaCaP:3. CCC (Vol% - - Cr2O3: 3%, - - - - - - by SEM) trace Cr2O3: trace Viscosity (Poise at - - 39 50 24 39 60.1 70.2 78.8 58.7 Processing Property 1150oC) Conductivity (S/cm at - - 0.19 0.16 0.39 0.2 0.16 0.16 0.24 0.22 1150oC) Quenched - - 9.265 9.305 3.714 7.583 5.367 3.995 0.474 1.517 Resistance PCT B (g/L) Leaching CCC PCTB - - 11.125 9.623 3.805 8.117 6.327 4.542 0.479 2.15 (g/L) TCLP - - PASS PASS PASS PASS PASS PASS PASS PASS (Pass/Fail) *: Estimated from XRD powder pattern analysis without an internal standard **: "VH": Very High, "H": High, "M": Medium; "-X": Letters after dash indicate component Sp: Spinel; LiP: Lithium phosphate; CaP: Calcium phosphate; NaCaP: Sodium calcium phosphate - Empty data field T-8 HFO-73169, Rev. 0 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.5. Viscosity and Electrical Conductivity of Selected HLW-HMn Glass Melts. HLW-HMn-9 HLW-HMn-10 HLW-HMn-13 Temperature (oC) Viscosity Conductivity Viscosity Conductivity Viscosity Conductivity (Poise) (S/cm) (Poise) (S/cm) (Poise) (S/cm) 1250 15.91 0.46 16.56 0.26 18.85 0.26 1150 32.14 0.34 33.71 0.17 39.43 0.19 1050 76.21 0.24 83.38 0.11 96.62 0.13 950 225.50 0.16 274.92 0.06 293.89 0.07 T-9 HFO-73169, Rev. 0 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.5. Viscosity and Electrical Conductivity of Selected HLW-HMn Glass Melts (continued). HLW-HMn-14 HLW-HMn-15 HLW-HMn-16 Temperature (oC) Viscosity Conductivity Viscosity Conductivity Viscosity Conductivity (Poise) (S/cm) (Poise) (S/cm) (Poise) (S/cm) 1250 23.65 0.22 12.06 0.52 19.09 0.27 1150 50.17 0.16 23.60 0.39 39.10 0.20 1050 128.42 0.11 54.51 0.28 96.00 0.13 950 430.04 0.06 159.42 0.19 305.87 0.07 T-10 HFO-73169, Rev. 0 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.5. Viscosity and Electrical Conductivity of Selected HLW-HMn Glass Melts (continued). HLW-HMn-17 HLW-HMn-18 HLW-HMn-19 HLW-HMn-20 Temperature (oC) Viscosity Conductivity Viscosity Conductivity Viscosity Conductivity Viscosity Conductivity (Poise) (S/cm) (Poise) (S/cm) (Poise) (S/cm) (Poise) (S/cm) 1250 27.26 0.21 30.95 0.22 35.17 0.32 26.86 0.28 1150 60.65 0.16 70.18 0.16 78.82 0.24 58.67 0.22 1050 163.26 0.10 192.54 0.10 211.33 0.17 154.33 0.15 950 574.31 0.05 688.86 0.06 724.99 0.11 527.22 0.07 T-11 HFO-73169, Rev. 0 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.6. PCT Releases of Selected HLW-HMn Glasses. Sample Normalized HLW- HLW- HLW- HLW- HLW- HLW- HLW- HLW- HLW- HLW- DWPF- Type PCT (g/L) HMn-9 HMn-10 HMn-13 HMn-14 HMn-15 HMn-16 HMn-17 HMn-18 HMn-19 HMn-20 EA B (g/L) 1.553 10.368 9.265 9.305 3.714 7.583 5.367 3.995 0.474 1.517 18.85 Quenched Li (g/L) 1.315 10.066 8.099 6.084 2.825 6.502 4.715 3.235 0.628 1.265 10.00 Sample Na (g/L) 3.244 2.213 0.242 0.941 13.64 0.790 7.599 5.627 5.664 1.799 4.817 Si (g/L) 0.352 0.276 0.146 0.146 0.364 0.202 0.147 0.143 0.276 0.204 3.99 B (g/L) 1.870 9.827 11.125 9.923 3.805 8.117 6.327 4.542 0.479 2.150 - CCC Li (g/L) 1.480 9.731 9.961 8.549 2.885 6.825 5.366 3.709 0.579 1.813 - Sample Na (g/L) 3.625 2.428 0.253 1.272 - 0.900 7.181 6.559 6.284 1.756 5.030 Si (g/L) 0.360 0.300 0.150 0.142 0.396 0.206 0.146 0.153 0.278 0.205 - - Empty data field T-12 HFO-73169, Rev. 0 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.7. TCLP Results (ppm) of Selected HLW-HMn Glasses. Element Ba Cd Cr Ni Pb UTS Limits 21 0.11 0.6 11 0.75 Delisting Limits 100 0.48 4.95 22.6 5 HLW-HMn-9 0.24 N/A 0.03 0.17 <0.10 HLW-HMn-10 0.47 N/A 0.17 1.09 0.30 HLW-HMn-13 0.32 N/A 0.07 0.36 0.15 HLW-HMn-14 0.23 N/A 0.04 0.19 0.11 HLW-HMn-15 0.23 N/A 0.05 0.22 <0.10 HLW-HMn-16 0.24 N/A 0.07 0.39 <0.10 HLW-HMn-17 0.26 N/A 0.04 0.25 <0.10 HLW-HMn-18 0.26 N/A 0.02 0.19 <0.10 HLW-HMn-19 0.23 N/A 0.02 0.10 <0.10 HLW-HMn-20 0.27 N/A 0.02 0.14 <0.10 N/A- Not Applicable (not present in glass) T-13 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.8. Composition (wt%) and Properties of High Manganese (Waste Batch 3939) HLW Simulant and Glass Formulation HLW-HMn-20 with 35% Waste Loading. Batch 3939 Glass Forming Target Glass Waste in Glass Waste Additives (HLW-HMn-20) Al2O3 31.09% 10.88% — 10.88% B 2O 3 0.30% 0.11% 16.00% 16.11% Bi2O3 4.33% 1.52% — 1.52% CaO 1.47% 0.51% — 0.51% Cr2O3 2.54% 0.89% — 0.89% F 0.25% 0.09% — 0.09% Fe2O3 9.37% 3.28% — 3.28% K2O 0.63% 0.22% 4.00% 4.22% La2O3 0.66% 0.23% — 0.23% Li2O — — 3.50% 3.50% MgO 0.40% 0.14% — 0.14% MnO 14.34% 5.02% — 5.02% Na2O 20.71% 7.25% — 7.25% Nd2O3 0.14% 0.05% — 0.05% NiO 1.92% 0.67% — 0.67% P 2O 5 2.97% 1.04% — 1.04% PbO 0.45% 0.16% — 0.16% SO3 0.98% 0.34% — 0.34% SiO2 6.57% 2.30% 38.50% 40.80% SrO 0.32% 0.11% — 0.11% Tl2O 0.18% 0.06% — 0.06% WO3 0.12% 0.04% — 0.04% ZrO2 0.25% 0.09% 3.00% 3.09% Total 100.0% 35.0% 65.00% 100.0% Viscosity @ 1150°C (P) 58.67 Electrical Conductivity @ 1150°C (S/cm) 0.22 Crystal Content, as melted (vol%) 0.5 Crystal Content, 70 hr at 950°C (vol%) 0.88 TCLP Pass Element DWPF-EA B 16.695 1.517 PCT (g/l) Li 9.565 1.265 Na 13.346 0.941 (1) — Empty data field. * Analyzed by SEM/EDS/Image Analysis T-14 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.9. Composition of Melter Feed to Produce 100 kg of Target Glass from High Manganese (Waste Batch 3939) HLW Simulant (Target Glass Yield = 500 g/l). Batch 3939 HLW Simulant Glass-Forming Additives Starting Materials Target Weight (kg)* Starting Materials Target Weight (kg) Al(OH)3 16.771 ─ ─ H3BO3 0.189 H3BO3 28.474 Bi2O3 1.526 ─ ─ CaCO3 0.928 ─ ─ Cr2O3 0.897 ─ ─ NaF 0.197 ─ ─ Fe(OH)3 Slurry (13%) 33.862 ─ ─ K2CO3 0.325 K2CO3 5.905 La2O3 0.239 ─ ─ ─ ─ Li2CO3 8.772 MgO 0.144 ─ ─ MnO 5.033 $ ─ ─ NaOH 5.763 ─ ─ Nd2O3 0.048 ─ ─ Ni(OH)2 0.839 ─ ─ Na3PO4 2.436 ─ ─ PbO 0.158 ─ ─ Na2SO4 0.614 SiO2 2.320 ─ ─ SrCO3 0.163 SiO2 37.343 Tl2O3 0.067 ─ ─ WO3 0.041 ─ ─ Zr(OH)4.xH2O 0.189 ZrSiO4 4.523 Na2CO3 1.548 ─ ─ NaNO2 0.006 ─ ─ NaNO3 0.379 ─ ─ H2C2O4·2H2O 0.049 ─ ─ Water 114.226 ─ ─ ─ ─ ─ ─ TOTAL 188.956 TOTAL 85.017 ─ ─ FEED TOTAL 273.973 Target weights adjusted for assay information of starting materials. – Empty data field. * $ - MnO2 6.214 kg or MnCO3 8.272 kg for appropriate tests T-15 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.10. Characteristics of Melter Feed Samples with the HLW-HMn-20 Formulation and Various Forms of Manganese. Glass Yield Manganese % Density Date Name pH Measured Target Source Water (g/ml) (g/l) %Dev. (kg/kg) (kg/kg) As-received, 11/10/16 XBL-F-8A 49.6 9.6 1.46 621 0.426 0.365 14.22 without 11/10/16 XBL-F-8B 49.6 9.7 1.47 629 0.428 0.365 14.74 manganese 11/14/16 XBL-F-19B 58.3 9.7 1.37 492 0.359 0.365 -1.59 MnO 11/18/16 XBL-F-58A 56.8 9.8 1.38 511 0.370 0.365 1.43 MnO2 11/29/16 XBL-F-79A 57.3 9.6 1.38 497 0.360 0.365 -1.45 MnCO3 12/1/2016 XBL-F-96A 55.8 9.7 1.39 512 0.368 0.363 1.47 T-16 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.11. XRF and DCP Analyzed Compositions of As-Received Vitrified Melter Feed Samples (wt%). Target XBL-F-8A XBL-F-8B Avg. % Dev. Al2O3 11.46 12.10 11.97 12.04 5.04 B2O3# 16.96 15.34 15.30 15.32 -9.66 Bi2O3 1.60 1.58 1.62 1.60 0.15 CaO 0.54 0.55 0.52 0.54 NC Cl & 0.01 0.02 0.02 NC Cr2O3 0.94 0.83 0.82 0.82 NC F$ 0.09 0.09 0.09 0.09 NC Fe2O3 3.45 3.68 3.68 3.68 6.58 K2O 4.44 4.09 4.14 4.11 -7.39 La2O3 0.24 0.18 0.18 0.18 NC Li2O# 3.68 3.23 3.20 3.22 -12.75 MgO 0.15 0.22 0.28 0.25 NC MnO & < 0.01 < 0.01 < 0.01 NC Na2O 7.63 7.30 7.40 7.35 -3.65 Nd2O3 0.05 0.05 0.05 0.05 NC NiO 0.71 0.77 0.73 0.75 NC P2O5 1.10 1.08 1.03 1.06 -3.47 PbO 0.17 0.17 0.17 0.17 NC SO3 0.36 0.30 0.35 0.33 NC SiO2 42.96 45.17 45.18 45.17 5.16 SrO 0.12 0.11 0.12 0.12 NC TiO2 & 0.04 0.03 0.03 NC Tl2O3 0.07 0.04 0.04 0.04 NC WO3 0.04 0.05 0.04 0.04 NC ZnO & 0.01 0.01 0.01 NC ZrO2 3.25 3.00 3.04 3.02 -7.13 Sum 100.00 100.00 100.00 100.00 # Measured by DCP-AES & Not a target constituent $ Target concentration T-17 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.12. XRF and DCP Analyzed Compositions of Vitrified Melter Feed Samples for the HLW-HMn20 Formulation and Various Forms of Manganese (wt%). XBL-F- XBL-F- XBL-F- XBL-F- Target Avg. % Dev. 19B 58A 79A 96A Al2O3 10.88 11.39 11.37 11.20 11.19 11.29 3.72 B2O3# 16.11 14.36 14.79 15.57 14.95 14.92 -7.38 Bi2O3 1.52 1.54 1.49 1.50 1.53 1.51 -0.22 CaO 0.51 0.51 0.52 0.50 0.49 0.51 NC Cl & 0.03 0.02 0.02 0.01 0.02 NC Cr2O3 0.89 0.84 0.73 0.83 0.85 0.81 NC F$ 0.09 0.09 0.09 0.09 0.09 0.09 NC Fe2O3 3.28 3.53 3.43 3.49 3.50 3.49 6.43 K2O 4.22 3.88 3.81 3.94 3.96 3.90 -7.58 La2O3 0.23 0.15 0.13 0.12 0.15 0.14 NC Li2O# 3.50 3.12 2.92 3.40 3.15 3.15 -10.07 MgO 0.14 0.21 0.27 0.23 0.23 0.24 NC MnO 5.02 4.83 4.87 4.89 4.78 4.84 -3.55 Na2O 7.25 7.12 7.01 6.65 6.90 6.92 -4.57 Nd2O3 0.05 0.06 0.05 0.06 0.05 0.05 NC NiO 0.67 0.73 0.68 0.71 0.74 0.71 NC P2O5 1.04 1.06 1.03 1.03 1.04 1.04 -0.31 PbO 0.16 0.16 0.16 0.15 0.17 0.16 NC SO3 0.34 0.26 0.25 0.32 0.28 0.28 NC SiO2 40.80 43.04 43.01 42.33 42.89 42.82 4.94 SrO 0.11 0.11 0.10 0.11 0.11 0.11 NC TiO2 & 0.04 0.04 0.02 0.03 0.03 NC Tl2O3 0.06 0.05 0.03 0.03 0.03 0.03 NC WO3 0.04 0.04 0.03 0.04 0.04 0.04 NC ZnO & < 0.01 0.01 < 0.01 0.01 0.01 NC ZrO2 3.09 2.84 3.16 2.78 2.84 2.91 -5.83 Sum 100.00 100.00 100.00 100.00 100.00 100.00 # Measured by DCP-AES & Not a target constituent $ Target concentration T-18 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 2.13. VGF Test Results for HLW-HMn-20 Formulation with Various Forms of Manganese Compared to Results for a High Iron Formulation with Different Iron Sources. Formulation Sample Test Ranking Definition XBL-F-19A (MnO) 1 Very Fast, all feed HLW-HMn-20 XBL-F-79A (MnO2) 3 Moderate with foamy High residue on side wall Manganese XBL-F-96A (MnCO3) 1 Very Fast, all feed Very Fast, all feed MnO 1 Very Fast, all feed MnCO3 1 HLW-HMn-10 Moderate with foamy High MnO2 3 residue on side wall Manganese Moderate with foamy MnO2 + 0.5 stoichiometric sugar 3 residue on side wall Very Fast, all feed MnO2 + 1.0 stoichiometric sugar 1 Moderate with foamy Iron Hydroxide Fe(OH)3 [16] 3 residue on side wall Very Fast, all feed Goethite/FeO(OH) [29] 1 HLW-NG-Fe2 Very Fast, all feed Hematite/Fe2O3 [29] 1 High Iron converted Magnetite/Fe3O4 [29] Very Fast, all feed 1 NOAH iron mixture [29] Very Fast, all feed 1 T-19 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 3.1. Summary of Results from DM100 Tests while Processing the HLW-HMn-20 Glass Composition and Various Manganese Sources. MnO, MnO, Test Optimized Nominal Bubbling Bubbling Feed Start 11/14/16 15:00 11/16/16 18:04 Time Feed End 11/16/16 18:00 11/18/16 20:00 Interval 51.0 hr 50.0 hr Water Feeding for Cold Cap 60 min 0 min Slurry Feeding 50.0 hr 50.0 hr Feeding Interruptions 19 min 6 min Average Bubbling Rate 14.5 lpm 9.0 lpm Used 965 kg 583 kg 500 g/l 500 g/l Feed Target Glass yield 0.365 kg/kg 0.365 kg/kg Average Feed Rate 19.3 kg/hr 11.7 kg/hr Poured 334 kg 207 kg Average Rate based on 1484 kg/m2/day 921 kg/m2/day Glass Produced glass poured Average Rate based on 1565 kg/m2/day 949 kg/m2/day feed consumed Steady State Rate* 1560 kg/m2/day 920 kg/m2/day 3.9 kW hr/kg 4.6 kW hr/kg Average Power Use glass glass *: Rates estimated from feed data. Note: Rates do not take into account the time for water feeding and cold cap burn-off. T-20 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 3.1. Summary of Results from DM100 Tests with the HLW-HMn-20 Glass Composition and Various Manganese Sources (continued). Test MnO2 MnCO3 Time Feed Start 11/28/16 11:16 11/30/16 15:30 Feed End 11/30/16 14:30 12/2/16 17:30 Interval 51.2 hr 50.0 hr Water Feeding for Cold Cap 102 min 0 min Slurry Feeding 49.7 hr 50.0 hr Feeding Interruptions 8 min 6 min Average Bubbling Rate 9.0 lpm 9.0 lpm Used 482 kg 497 kg 500 g/l 500 g/l Feed Target Glass yield 0.365 kg/kg 0.363 kg/kg Average Feed Rate 9.7 kg/hr 9.9 kg/hr Poured 171 kg 185 kg Average Rate based on 763 kg/m2/day 824 kg/m2/day Glass Produced glass poured Average Rate based on 788 kg/m2/day 801 kg/m2/day feed consumed Steady State Rate* 750 kg/m2/day 800 kg/m2/day 5.2 kW hr/kg 5.1 kW hr/kg Average Power Use glass glass *: Rates estimated from feed data. Note: Rates do not take into account the time for water feeding and cold cap burn-off. T-21 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 3.2. Steady-State Production Rates Achieved on the DM100 Melter with Various Hanford HLW Streams at a Glass Temperature of 1150oC and Feed Solids Content of 500 g Glass Per Liter. Glass Waste Melt Pool Production Glass Formulation Loading Bubbling (lpm) Rate (wt% Oxide) (kg/m2/day) HLW-HMn-20 9.0 920 (Mn Limited, MnO as 35 Manganese Source, Present Work) Optimized, 14.5 1560 9.0 1100 HLW-HP-16 [32] 51 (P Limited) Optimized, 15.8 1600 9.1 1280 HLW-Zr-11[22] 33 (Zr Limited) Optimized, 14.6 1740 9.3 1400 HLW-HSr-7r [21] 55 (Sr Limited) Optimized, 14.6 1600 9.0 1100 HLW-HCr-16 [20] 45 (Cr Limited) Optimized, 15.6 1550 8.9 1650 HLW-NG-Fe2 [16] 42 (Fe Limited) Optimized, 13.2 1900 8.8 1660 HLW-Bi-F9 [17] 50 (Bi Limited) Optimized, 10.0 2000 HWI-Al-28 [27] 50 8.9 1900 (Al Limited) T-22 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 3.3. Steady-State Production Rates Achieved with Iron and Manganese Limited HLW Compositions and Different Forms of the Waste Loading Limiting Components. DM100 at Melt Pool Bubbling of 9 lpm and Solids content of 500 g glass/liter. Increase/Decrease Production Over Reduced Form of Waste Loading Glass Formulation Rate Metal Oxide Limiting Component kg/m2/day 2 kg/m /day Percent MnO 920 - - HLW-HMn-20 MnCO3 800 -120 -13% MnO2 750 -170 -18% Magnetite [29] 1830 - - Goethite [29] 1725 -105 -5.7% HLW-NG-Fe2 Hematite [29] 1910 80 4.4% Fe(OH)3 [16] 1650 -180 -9.8% - Empty data field T-23 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 3.4. Summary of Measured DM100 Parameters while Processing the HLW-HMn-20 Glass Composition and Various Manganese Sources. MnO, Optimized Bubbling MnO, Nominal Bubbling Test AVG MIN MAX AVG MIN MAX East Upper 1028 953 1045 1002 984 1034 T Electrode West Upper 933 897 974 921 884 945 E West Lower 1075 1046 1087 1061 1046 1085 M Bottom 697 662 718 703 695 717 P 27” from bottom 1138 1024 1165 1129 1053 1167 E 16” from bottom 1146 1102 1170 1147 1114 1171 R Glass 10” from bottom 1156 1125 1176 1163 1148 1179 A T 5” from bottom 1153 1128 1171 1155 1134 1174 U Exposed 476 386 690 424 374 463 Plenum R Thermowell 461 373 692 424 373 461 E Discharge Chamber 1048 1007 1073 1049 1015 1072 (oC) Film Cooler Outlet 279 273 287 278 271 283 Transition Line Outlet 264 255 279 263 259 269 Lance Bubbling (lpm) 14.5 3.3 17.1 9.0 8.9 17.1 Melter Pressure (inches water) -0.85 -2.46 0.19 -0.84 -1.81 0.04 Total Electrode Voltage (V) 44.6 30.5 52.1 44.6 40.4 49.4 Total Electrode Power (kW) 26.0 20.4 28.6 19.1 17.8 25.5 Glass Resistance (ohms) 0.077 0.044 0.108 0.104 0.090 0.113 T-24 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 3.4. Summary of Measured DM100 Parameters while Processing the HLW-HMn-20 Glass Composition and Various Manganese Sources (continued). MnO2 MnCO3 Test AVG MIN MAX AVG MIN MAX East Upper 1001 975 1014 1007 987 1018 T Electrode West Upper 934 891 980 928 904 947 E West Lower 1064 1051 1075 1057 1048 1070 M Bottom 708 684 720 718 715 722 P 27” from bottom 1136 1101 1159 1142 1093 1158 E 16” from bottom 1139 1107 1159 1137 1115 1163 R Glass 10” from bottom 1161 1149 1171 1158 1145 1172 A T 5” from bottom 1154 1130 1167 1151 1139 1165 U Exposed 483 387 678 475 440 509 Plenum R Thermowell 475 358 680 479 427 525 E Discharge Chamber 1042 1001 1065 1053 1012 1075 (oC) Film Cooler Outlet 278 272 286 278 270 284 Transition Line Outlet 264 242 267 263 258 265 Lance Bubbling (lpm) 9.0 1.3 9.3 9.0 8.9 9.3 Melter Pressure (inches water) -0.86 -2.41 0.05 -0.90 -1.23 0.05 Total Electrode Voltage (V) 43.3 41.2 46.6 44.1 37.9 45.4 Total Electrode Power (kW) 17.9 16.7 19.9 18.7 14.2 19.1 Glass Resistance (ohms) 0.105 0.101 0.112 0.104 0.101 0.111 T-25 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 4.1. List of Glass Discharged and Masses During Tests with the HLW-HMn-20 Formulation and Various Forms of Manganese. Cumulative Mass Test Date Sample Name Discharge (kg) (kg) XBL-G-18A 35.02 35.02 XBL-G-18B 11/14/2016 XBL-G-19A 19.04 54.06 XBL-G-19B XBL-G-19C 25.94 80.00 XBL-G-19D XBL-G-21A 18.26 98.26 XBL-G-21B XBL-G-21C 26.68 124.94 XBL-G-21D 11/15/2016 XBL-G-21E 30.96 155.90 XBL-G-25A MnO, XBL-G-25B optimized 22.62 178.52 bubbling XBL-G-28A XBL-G-28B 24.16 202.68 XBL-G-29A XBL-G-29B 24.50 227.18 XBL-G-29C XBL-G-29D 28.14 255.32 XBL-G-34A XBL-G-34B 28.06 283.38 11/16/2016 XBL-G-34C XBL-G-34D 24.76 308.14 XBL-G-36A XBL-G-36B 25.42 333.56 XBL-G-36C T-26 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 4.1. List of Glass Discharged and Masses During Tests with the HLW-HMn-20 Formulation and Various Forms of Manganese (continued). Cumulative Mass Test Date Sample Name Discharge (kg) (kg) 11/16/2016 XBL-G-39A 27.14 27.14 XBL-G-39B XBL-G-40A 28.90 56.04 XBL-G-40B 11/17/2016 XBL-G-40C 26.16 82.20 XBL-G-40D XBL-G-49A 28.58 110.78 MnO, nominal XBL-G-49B XBL-G-49C 27.40 138.18 XBL-G-50A XBL-G-50B 28.60 166.78 11/18/2016 XBL-G-50C XBL-G-50D 25.24 192.02 XBL-G-50E XBL-G-58A 14.28 206.30 XBL-G-75A 19.94 19.94 XBL-G-75B 11/28/2016 XBL-G-75C 21.58 41.52 XBL-G-79A XBL-G-79B 20.82 62.34 XBL-G-79C XBL-G-79D 20.00 82.34 XBL-G-81A 11/29/2016 XBL-G-81B MnO2 18.58 100.92 XBL-G-81C XBL-G-81D 19.50 120.42 XBL-G-85A XBL-G-85B 18.10 138.52 XBL-G-85C XBL-G-85D 11/30/2016 17.10 155.62 XBL-G-89A XBL-G-89B 15.00 170.62 XBL-G-89C T-27 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 4.1. List of Glass Discharged and Masses During Tests with the HLW-HMn-20 Formulation and Various Forms of Manganese (continued). Cumulative Mass Test Date Sample Name Discharge (kg) (kg) XBL-G-94A 20.18 20.18 11/30/2016 XBL-G-94B XBL-G-96A 21.70 41.88 XBL-G-96B XBL-G-96C 19.34 61.22 XBL-G-96D 12/1/2016 XBL-G-100A 25.98 87.20 XBL-G-100B MnCO3 XBL-G-100C 26.62 113.82 XBL-G-100D XBL-G-105A 22.26 136.08 XBL-G-105B XBL-G-105C 12/2/2016 23.12 159.20 XBL-G-105D XBL-G-105E 26.20 185.40 XBL-G-113A T-28 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 4.2. XRF Analyzed Composition of Glass Discharged During DM100 Testing with the HLW-HMn-20 Glass Composition and MnO as the Manganese Source (wt%). Glass 35.02 54.06 80.00 98.26 124.94 155.90 178.52 (kg) Constituents XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- Target 18B 19B 19D 21B 21D 25A 28A Al2O3 10.88 13.25 13.09 13.04 12.65 12.41 12.21 12.10 B2O3# 16.11 11.82 12.13 12.51 12.74 13.04 13.34 13.52 Bi2O3 1.52 2.91 2.67 2.54 2.41 2.27 2.13 2.13 CaO 0.51 1.16 1.08 1.02 0.98 0.89 0.85 0.80 Cl & 0.02 0.02 0.01 0.01 0.01 0.01 0.02 Cr2O3 0.89 0.77 0.76 0.71 0.71 0.71 0.73 0.72 F$ 0.09 0.08 0.08 0.07 0.07 0.06 0.06 0.05 Fe2O3 3.28 6.17 5.76 5.53 5.24 4.97 4.71 4.70 K2O 4.22 0.59 0.94 1.28 1.60 1.98 2.35 2.56 La2O3 0.23 < 0.01 0.04 0.06 0.07 0.11 0.10 0.11 Li2O# 3.50 0.64 0.89 1.19 1.38 1.63 1.87 2.02 MgO 0.14 0.10 0.14 0.14 0.13 0.17 0.17 0.20 MnO 5.02 1.29 1.69 1.97 2.28 2.81 3.01 3.38 Na2O 7.25 19.15 18.20 17.09 15.64 14.08 13.23 12.23 Nd2O3 0.05 < 0.01 < 0.01 < 0.01 0.02 < 0.01 0.03 < 0.01 NiO 0.67 0.73 0.73 0.72 0.71 0.71 0.70 0.70 P2O5 1.04 6.39 5.65 5.13 4.69 4.05 3.57 3.25 PbO 0.16 0.25 0.23 0.22 0.22 0.21 0.19 0.21 SO3 0.34 0.55 0.49 0.47 0.45 0.36 0.36 0.31 SiO2 40.80 33.56 34.60 35.27 36.67 37.88 38.51 38.87 SrO 0.11 0.13 0.12 0.12 0.13 0.12 0.12 0.12 TiO2 & 0.01 < 0.01 0.02 0.02 0.01 0.01 0.03 Tl2O3 0.06 0.01 0.01 0.02 0.02 0.03 0.02 0.03 WO3 0.04 < 0.01 < 0.01 < 0.01 0.02 0.03 0.03 0.03 ZnO & 0.01 0.01 0.01 0.01 0.01 0.01 0.01 ZrO2 3.09 0.41 0.67 0.87 1.13 1.45 1.69 1.89 Sum 100.00 100.00 100.00 100.00 100.00 100.00 100.00 100.00 & - Not a target constituent # - B2O3 and Li2O concentrations calculated from DCP-AES analysis of glass in the melt pool prior to the tests (XBL-D-8A) and T-29 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 4.2. XRF Analyzed Composition of Glass Discharged During DM100 Testing with the HLW- HMn-20 Glass Composition and MnO as the Manganese Source (wt%) (continued). Glass (kg) 202.68 227.18 255.32 283.38 308.14 333.56 Constituents XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- Target 29A 29C 34A 34C 36A 36C Al2O3 10.88 12.15 12.01 11.88 11.84 11.73 11.74 B2O3# 16.11 13.70 13.85 14.01 14.14 14.24 14.33 Bi2O3 1.52 1.94 1.89 1.91 1.82 1.71 1.70 CaO 0.51 0.74 0.71 0.64 0.69 0.62 0.61 Cl & 0.01 0.01 0.01 0.01 0.01 0.01 Cr2O3 0.89 0.70 0.71 0.74 0.75 0.71 0.74 F$ 0.09 0.05 0.05 0.05 0.04 0.04 0.04 Fe2O3 3.28 4.37 4.13 4.19 4.09 3.88 3.80 K2O 4.22 2.70 2.88 3.14 3.13 3.14 3.23 La2O3 0.23 0.10 0.12 0.11 0.15 0.10 0.13 Li2O# 3.50 2.16 2.28 2.41 2.52 2.60 2.67 MgO 0.14 0.21 0.19 0.21 0.18 0.23 0.23 MnO 5.02 3.44 3.64 3.93 4.03 4.05 4.20 Na2O 7.25 11.57 11.29 10.09 9.95 9.57 9.41 Nd2O3 0.05 0.04 0.04 0.03 0.03 0.06 0.06 NiO 0.67 0.70 0.70 0.74 0.72 0.71 0.68 P2O5 1.04 2.94 2.59 2.38 2.19 2.05 1.90 PbO 0.16 0.18 0.18 0.19 0.17 0.15 0.17 SO3 0.34 0.31 0.30 0.25 0.28 0.27 0.24 SiO2 40.80 39.84 40.16 40.59 40.68 41.51 41.45 SrO 0.11 0.11 0.11 0.12 0.11 0.11 0.11 TiO2 & 0.03 0.02 0.02 0.03 0.03 0.03 Tl2O3 0.06 0.03 0.03 0.03 0.03 0.02 0.03 WO3 0.04 0.03 0.03 0.04 0.04 0.03 0.05 ZnO & 0.01 0.01 0.01 0.01 0.01 0.01 ZrO2 3.09 1.95 2.07 2.28 2.37 2.39 2.45 Sum 100.00 100.00 100.00 100.00 100.00 100.00 100.00 & - Not a target constituent # - B2O3 and Li2O concentrations calculated from DCP-AES analysis of glass in the melt pool prior to the tests (XBL-D-8A) and T-30 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 4.2. XRF Analyzed Composition of Glass Discharged During DM100 Testing with the HLW-HMn-20 Glass Composition and MnO as the Manganese Source (wt%) (continued). Glass (kg) 360.70 389.60 415.76 444.34 471.74 500.34 525.58 539.86 Constituents XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- Target 39B 40B 40D 49B 50A 50C 50E 58A Al2O3 10.88 11.63 11.59 11.67 11.58 11.46 11.38 11.51 11.37 B2O3# 16.11 14.41 14.49 14.54 14.60 14.64 14.68 14.71 14.73 Bi2O3 1.52 1.69 1.68 1.56 1.65 1.60 1.64 1.55 1.60 CaO 0.51 0.62 0.64 0.53 0.54 0.55 0.54 0.56 0.54 Cl & 0.02 0.01 0.01 0.02 0.01 0.02 0.01 0.01 Cr2O3 0.89 0.75 0.76 0.76 0.78 0.77 0.79 0.73 0.76 F$ 0.09 0.04 0.04 0.04 0.04 0.04 0.03 0.03 0.03 Fe2O3 3.28 3.87 3.78 3.57 3.70 3.62 3.63 3.50 3.49 K2O 4.22 3.38 3.48 3.44 3.69 3.63 3.69 3.67 3.78 La2O3 0.23 0.17 0.16 0.18 0.17 0.20 0.21 0.15 0.15 Li2O# 3.50 2.74 2.80 2.84 2.89 2.93 2.96 2.98 3.00 MgO 0.14 0.22 0.21 0.25 0.25 0.22 0.24 0.24 0.27 MnO 5.02 4.28 4.46 4.36 4.54 4.54 4.62 4.53 4.63 Na2O 7.25 8.68 8.58 8.71 8.07 7.94 7.84 8.02 7.75 Nd2O3 0.05 0.06 0.05 0.04 0.05 0.04 0.06 0.05 0.07 NiO 0.67 0.73 0.73 0.67 0.71 0.70 0.73 0.72 0.69 P2O5 1.04 1.74 1.65 1.56 1.48 1.43 1.33 1.31 1.30 PbO 0.16 0.17 0.16 0.16 0.17 0.17 0.18 0.17 0.16 SO3 0.34 0.24 0.24 0.23 0.25 0.23 0.23 0.22 0.22 SiO2 40.80 41.81 41.61 42.13 41.92 42.28 42.17 42.41 42.46 SrO 0.11 0.11 0.11 0.11 0.11 0.11 0.11 0.11 0.10 TiO2 & 0.02 0.02 0.03 0.03 0.03 0.03 0.03 0.02 Tl2O3 0.06 0.03 0.04 0.03 0.03 0.04 0.04 0.04 0.03 WO3 0.04 0.04 0.04 0.03 0.03 0.04 0.05 0.04 0.03 ZnO & 0.01 0.01 0.01 0.01 0.00 0.00 0.01 0.01 ZrO2 3.09 2.55 2.65 2.53 2.71 2.76 2.82 2.70 2.78 Sum 100.00 100.00 100.00 100.00 100.00 100.00 100.00 100.00 100.00 & - Not a target constituent # - B2O3 and Li2O concentrations calculated from DCP-AES analysis of glass in the melt pool prior to the tests (XBL-D-8A) and T-31 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 4.3. XRF Analyzed Composition of Glass Discharged During DM100 Testing with the HLW-HMn-20 Glass Composition and MnO2 as the Manganese Source (wt%). Glass (kg) 559.80 581.38 602.20 622.20 640.78 660.28 678.38 695.48 710.48 Constituents XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- XBL- XBL- Target XBL-G-75B XBL-G-79A 79C 81A 81C 85A 85C G-89A G-89C Al2O3 10.88 11.52 11.48 11.40 11.41 11.39 11.33 11.36 11.29 11.35 B2O3# 16.11 14.75 14.77 14.79 14.80 14.81 14.82 14.83 14.84 14.84 Bi2O3 1.52 1.53 1.55 1.61 1.57 1.55 1.56 1.53 1.56 1.52 CaO 0.51 0.51 0.53 0.54 0.53 0.54 0.51 0.54 0.53 0.52 Cl & 0.01 < 0.01 0.01 0.01 0.01 0.01 0.01 0.01 0.01 Cr2O3 0.89 0.83 0.82 0.86 0.82 0.78 0.84 0.76 0.76 0.80 F$ 0.09 0.03 0.03 0.03 0.03 0.03 0.03 0.03 0.03 0.03 Fe2O3 3.28 3.58 3.60 3.61 3.58 3.54 3.53 3.50 3.53 3.42 K2O 4.22 3.60 3.73 3.77 3.68 3.64 3.77 3.81 3.84 3.68 La2O3 0.23 0.18 0.15 0.17 0.16 0.17 0.17 0.19 0.18 0.20 Li2O# 3.50 3.01 3.03 3.04 3.05 3.06 3.07 3.08 3.08 3.09 MgO 0.14 0.25 0.25 0.24 0.24 0.25 0.24 0.24 0.23 0.26 MnO 5.02 4.41 4.53 4.67 4.60 4.46 4.54 4.54 4.62 4.63 Na2O 7.25 7.67 7.68 7.36 7.74 7.49 7.46 7.41 7.24 7.44 Nd2O3 0.05 0.04 0.04 0.06 0.05 0.04 0.05 0.05 0.08 0.04 NiO 0.67 0.73 0.75 0.78 0.75 0.73 0.74 0.76 0.78 0.72 P2O5 1.04 1.32 1.28 1.30 1.28 1.29 1.23 1.25 1.23 1.20 PbO 0.16 0.16 0.16 0.17 0.16 0.16 0.16 0.15 0.16 0.16 SO3 0.34 0.20 0.19 0.18 0.22 0.18 0.18 0.21 0.20 0.18 SiO2 40.80 42.80 42.45 42.37 42.31 42.94 42.77 42.78 42.79 42.91 SrO 0.11 0.10 0.11 0.11 0.11 0.11 0.11 0.11 0.11 0.11 TiO2 & 0.03 0.03 0.03 0.03 0.02 0.03 0.03 0.03 0.03 Tl2O3 0.06 0.02 0.02 0.02 0.03 0.04 0.03 0.03 0.03 0.03 WO3 0.04 0.04 0.04 0.05 0.04 0.04 0.04 0.04 0.05 0.04 ZnO & 0.01 0.01 0.01 0.01 0.01 0.01 0.01 0.01 0.01 ZrO2 3.09 2.66 2.76 2.83 2.78 2.73 2.77 2.74 2.79 2.78 Sum 100.00 100.00 100.00 100.00 100.00 100.00 100.00 100.00 100.00 100.00 & - Not a target constituent # - B2O3 and Li2O concentrations calculated from DCP-AES analysis of glass in the melt pool prior to the tests (XBL-D-8A) and T-32 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 4.4. XRF Analyzed Composition for Glass Discharged During DM100 Testing with the HLW-HMn-20 Glass Composition and MnCO3 as the Manganese Source (wt%). Glass 730.66 752.36 771.70 797.68 824.30 846.56 869.68 895.88 (kg) Constituents XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- XBL-G- Target 94B 96B 96D 100B 100D 105B 105D 113A Al2O3 10.88 11.26 11.24 11.41 11.36 11.37 11.26 11.46 11.36 B2O3# 16.11 14.85 14.86 14.87 14.87 14.88 14.88 14.89 14.89 Bi2O3 1.52 1.58 1.54 1.51 1.49 1.50 1.54 1.49 1.56 CaO 0.51 0.52 0.52 0.52 0.52 0.54 0.52 0.51 0.53 Cl & 0.01 0.01 0.01 0.01 < 0.01 0.02 0.01 0.01 Cr2O3 0.89 0.82 0.79 0.75 0.77 0.79 0.77 0.77 0.80 F$ 0.09 0.03 0.03 0.03 0.03 0.03 0.03 0.03 0.03 Fe2O3 3.28 3.56 3.48 3.45 3.43 3.42 3.51 3.36 3.58 K2O 4.22 3.85 3.83 3.74 3.89 3.87 3.88 3.89 3.92 La2O3 0.23 0.19 0.20 0.19 0.16 0.16 0.20 0.17 0.12 Li2O# 3.50 3.09 3.10 3.11 3.11 3.12 3.12 3.12 3.13 MgO 0.14 0.24 0.25 0.24 0.24 0.24 0.24 0.26 0.25 MnO 5.02 4.71 4.70 4.53 4.63 4.63 4.72 4.70 4.78 Na2O 7.25 7.40 7.15 7.45 7.19 7.27 6.97 7.30 6.96 Nd2O3 0.05 0.04 0.05 0.05 0.04 0.05 0.05 0.05 0.04 NiO 0.67 0.76 0.73 0.72 0.73 0.71 0.71 0.69 0.74 P2O5 1.04 1.19 1.18 1.18 1.16 1.15 1.17 1.12 1.13 PbO 0.16 0.16 0.16 0.16 0.16 0.16 0.16 0.16 0.18 SO3 0.34 0.20 0.19 0.20 0.20 0.20 0.19 0.20 0.19 SiO2 40.80 42.43 42.94 42.90 43.00 42.94 42.95 42.82 42.69 SrO 0.11 0.11 0.11 0.11 0.10 0.11 0.11 0.11 0.12 TiO2 & 0.04 0.04 0.03 0.03 0.02 0.03 0.03 0.03 Tl2O3 0.06 0.04 0.03 0.04 0.03 0.04 0.04 0.04 0.03 WO3 0.04 0.04 0.03 0.04 0.04 0.04 0.04 0.04 0.04 ZnO & 0.01 0.01 0.01 0.01 0.01 0.01 0.01 0.01 ZrO2 3.09 2.85 2.83 2.76 2.79 2.76 2.86 2.78 2.90 Sum 100.00 100.00 100.00 100.00 100.00 100.00 100.00 100.00 100.00 & - Not a target constituent # - B2O3 and Li2O concentrations calculated from DCP-AES analysis of glass in the melt pool prior to the tests (XBL-D-8A) and average analyzed feed sample values using a simple well-stirred tank model T-33 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 4.5. XRF Analyzed Composition of Dip Samples Taken After DM100 Melter Tests (wt%). Prior to Prior to testing MnO MnO2 MnO2 MnCO3 Target testing XBL- XBL-D- XBL-D- XBL-D- XBL-D- D-8A 58A 66A 94A 113A Al2O3 10.88 13.45 11.45 11.43 11.41 11.19 B2O3# 16.11 11.16 14.18 14.56 13.92 15.28 Bi2O3 1.52 3.28 1.60 1.63 1.54 1.52 CaO 0.51 1.30 0.57 0.58 0.55 0.52 Cl & 0.01 0.01 < 0.01 < 0.01 0.01 Cr2O3 0.89 0.81 0.85 0.85 0.85 0.92 F$ 0.09 0.08 0.03 0.03 0.03 0.03 Fe2O3 3.28 6.75 3.62 3.76 3.53 3.57 K2O 4.22 0.13 3.75 3.72 3.90 3.95 La2O3 0.23 < 0.01 0.19 0.16 0.19 0.15 Li2O# 3.50 0.10 2.98 3.00 3.08 3.16 MgO 0.14 0.09 0.20 0.24 0.26 0.25 MnO 5.02 0.86 4.69 4.67 4.67 4.72 Na2O 7.25 20.89 7.78 7.67 7.46 6.84 Nd2O3 0.05 < 0.01 0.07 0.06 0.06 0.03 NiO 0.67 0.77 0.72 0.82 0.73 0.75 P2O5 1.04 6.99 1.29 1.37 1.24 1.09 PbO 0.16 0.28 0.17 0.17 0.16 0.16 SO3 0.34 0.58 0.33 0.18 0.21 0.21 SiO2 40.80 32.27 42.47 42.05 43.22 42.62 SrO 0.11 0.14 0.11 0.11 0.11 0.11 TiO2 & < 0.01 0.03 0.04 0.03 0.03 Tl2O3 0.06 < 0.01 0.04 0.03 0.03 0.03 WO3 0.04 < 0.01 0.05 0.06 0.04 0.05 ZnO & 0.01 0.01 0.01 0.01 0.01 ZrO2 3.09 0.06 2.81 2.81 2.78 2.79 Sum 100.00 100.00 100.00 100.00 100.00 100.00 # Measured by DCP-AES $ Estimated from measurements of solid samples by XRF & Not a target constituent T-34 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 4.6. Comparison of XRF Analysis of Terminal Discharged Glass from each Test and Target Composition. MnO, Optimized MnO, Nominal MnO2 MnCO3 Target Bubbling Bubbling XBL-G- XBL-G- XBL-G- XBL-G- % Dev. % Dev. % Dev. % Dev. 36C 58A 89C 113A Al2O3 10.88 11.74 7.88 11.37 4.48 11.35 4.33 11.36 4.38 # B2O3 16.11 14.33 NC 14.73 NC 14.84 NC 14.89 NC Bi2O3 1.52 1.70 12.37 1.60 5.40 1.52 0.29 1.56 2.93 CaO 0.51 0.61 NC 0.54 NC 0.52 NC 0.53 NC Cl & 0.01 NC 0.01 NC 0.01 NC 0.01 NC Cr2O3 0.89 0.74 NC 0.76 NC 0.80 NC 0.80 NC $ F 0.09 0.04 NC 0.03 NC 0.03 NC 0.03 NC Fe2O3 3.28 3.80 15.77 3.49 6.57 3.42 4.31 3.58 9.24 K2O 4.22 3.23 -23.48 3.78 -10.52 3.68 -12.90 3.92 -7.11 La2O3 0.23 0.13 NC 0.15 NC 0.20 NC 0.12 NC # Li2O 3.50 2.67 NC 3.00 NC 3.09 NC 3.13 NC MgO 0.14 0.23 NC 0.27 NC 0.26 NC 0.25 NC MnO 5.02 4.20 -16.33 4.63 -7.70 4.63 -7.74 4.78 -4.80 Na2O 7.25 9.41 29.77 7.75 6.96 7.44 2.66 6.96 -4.02 Nd2O3 0.05 0.06 NC 0.07 NC 0.04 NC 0.04 NC NiO 0.67 0.68 NC 0.69 NC 0.72 NC 0.74 NC P2O5 1.04 1.90 82.69 1.30 25.09 1.20 15.25 1.13 8.22 PbO 0.16 0.17 NC 0.16 NC 0.16 NC 0.18 NC SO3 0.34 0.24 NC 0.22 NC 0.18 NC 0.19 NC SiO2 40.80 41.45 1.59 42.46 4.07 42.91 5.16 42.69 4.62 SrO 0.11 0.11 NC 0.10 NC 0.11 NC 0.12 NC TiO2 & 0.03 NC 0.02 NC 0.03 NC 0.03 NC Tl2O3 0.06 0.03 NC 0.03 NC 0.03 NC 0.03 NC WO3 0.04 0.05 NC 0.03 NC 0.04 NC 0.04 NC ZnO & 0.01 NC 0.01 NC 0.01 NC 0.01 NC ZrO2 3.09 2.45 -20.79 2.78 -9.98 2.78 -10.01 2.90 -6.05 Sum 100.00 100.00 - 100.00 - 100.00 - 100.00 - # B2O3 and Li2O concentrations calculated from DCP-AES analysis of glass in the melt pool prior to the tests (XBL-D-8A) and & Not a target constituent. NC - Not calculated - Empty data field T-35 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 4.7. PCT Releases for Melter and Crucible Glasses (ASTM C 1285, 7-days at 90ºC, Stainless Steel Vessel; S/V=2000 m-1). Crucible Melter Glass Melter Glass Melter Glass Glass Glass HLW- DWPF-EA XBL-G-58A XBL-G-89C XBL-G-113A HMn-20 B 44.71 35.52 46.19 PCT Li 8.26 8.94 12.2 Concentrations Na 38.69 33.34 38.21 (mg/l) Si 32.19 39.55 39.50 B 0.89 0.71 0.92 1.52 16.695 PCT Li 0.51 0.55 0.75 1.27 9.565 Normalized Na 0.69 0.59 0.68 0.94 13.346 Concentrations Si 0.17 0.20 0.20 0.20 3.922 (g/l) pH 9.40 9.55 9.53 9.61 11.85 PCT B 0.45 0.36 0.46 Normalized Li 0.26 0.28 0.38 Mass Loss Na 0.35 0.30 0.34 (g/m2) Si 0.09 0.10 0.10 Table 4.8. TCLP Results for Melter and Crucible Glasses (mg/l). Element Cr Ni Pb Mn UTS Limits# 0.60 11.00 0.75 NRL Delisting Limits 4.95 22.6 5.00 NRL [52, 53] Melter Glass 0.02 0.16 0.13 1.74 XBL-G-58A Melter Glass 0.02 0.09 0.40 1.94 XBL-G-89C Melter Glass 0.01 0.18 0.46 2.08 XBL-G-113A Crucible Glass HLW-HMn-20 0.02 0.14 <0.10 1.31 # For comparison only; does not apply to WTP glasses NRL – No regulatory limit T-36 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 4.9. Volume Percent Spinels and Mössbauer Analysis of Melter Glasses. Mössbauer Volume % Spinels Sample Name Sampling Time (% of total iron) XRD SEM 98.3% Fe+3 XBL-D-8A Pretest Melt Pool sample < 0.1 NM 1.7% Fe+2 Discharge Glass after XBL-G-58A 100% Fe+3 1.0 0.70 tests with MnO Melt Pool sample after XBL-D-58A 100% Fe+3 0.9 NM tests with MnO XBL-D-66A Pretest Melt Pool sample 100% Fe+3 0.9 NM Discharge Glass after XBL-G-89C 100% Fe+3 0.8 0.83 tests with MnO2 Melt Pool sample after 98.8% Fe+3 XBL-D-94A 0.6 NM tests with MnO2 1.2% Fe+2 Discharge Glass after 98.4% Fe+3 XBL-G-113A 1.1 0.75 tests with MnCO3 1.6% Fe+2 Melt Pool sample after 95.6% Fe+3 XBL-D-113A 0.8 NM tests with MnCO3 4.4% Fe+2 NM – Not measured Table 4.10. Description of Crystalline Phases Identified by SEM. Sample Sampling Secondary Phase Description Name Time NiFeMnCr-spinels are sub-euhedral, granular, mostly 5-20 micron size, a few Discharge down to 1 micron size, clustered, and heterogeneously distributed in the XBL-G- glass after sample. The chemical composition of NiFeMnCr-spinel is slightly variable 58A tests with with trace amounts of Fe enriched spinel also observed. Cr-oxide is trace level, MnO sub-anhedral, and exists as the core of some spinel clusters. CrMnNiFe-spinel is euhedral, granular, mostly 5-60 micron size, heavily Discharge clustered or locally concentrated, some hollow skeletal, and highly glass after heterogeneously distributed in the sample. The chemical composition of the XBL-G-89C test with crystal is variable. The crystal contains small amounts of Al-Zn and possibly MnO2 Ti-Cd-Si. EDS analysis indicates that the large spinel crystal contains slightly higher Fe-Ni, while smaller spinel is slightly higher in Cr-Mn. NiFeMnCr-spinel is sub-euhedral, granular, mostly 5-20 micron size, a few Discharge down to 1 micron size, clustered, and heterogeneously distributed in the XBL-G- glass after sample. The chemical composition of NiFeMnCr-spinel is slightly variable. 113A test with Trace amount Fe enriched spinel, some over 100 micron size are observed in MnCO3 the sample. Cr-oxide is trace level, sub-anhedral, and exists as the core of some spinel clusters. T-37 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 5.1. Results from DM100 Off-Gas Emission Samples while Processing the HLW-HMn-20 Glass Composition and Various Manganese Sources. MnO, Optimized MnO, Nominal 11/16/2016 11:27 – 12:27 11/17/2016 15:33 – 16:33 14.7% Moisture, 105% Isokinetic 9.27% Moisture, 96.6% Isokinetic Feed# Output % Feed# Output % DF DF (mg/min) (mg/min) Emitted (mg/min) (mg/min) Emitted $ Total 134296 453 0.34 296 84318 195 0.23 432 Al 6759 13.9 0.21 485 4098 3.67 0.09 1118 B 5869 32.3 0.55 182 3558 10.6 0.30 334 Bi 1597 8.23 0.52 194 968 2.88 0.30 336 Ca 431 1.37 0.32 315 261 0.47 0.18 561 Cr 715 3.23 0.45 221 434 2.61 0.60 166 F* 103 14.4 14.0 7.16 62.5 5.25 8.39 11.9 Fe 2692 10.4 0.39 259 1632 2.95 0.18 553 K 4113 30.7 0.75 133.9 2493 12.95 0.52 192.5 La 231 < 0.10 < 0.04 > 2313 140 < 0.10 < 0.07 > 1402 Li 1909 5.31 0.28 360 1157 1.85 0.16 626 Particulate Mg 98.6 0.52 0.53 189 59.8 0.17 0.28 362 Mn 4565 15.22 0.33 300 2767 4.15 0.15 667 Na 6313 35.7 0.56 177 3827 11.8 0.31 324 Nd 112 < 0.10 < 0.09 > 1118 67.8 < 0.10 < 0.15 > 678 Ni 619 0.94 0.15 659 375 0.22 0.06 1716 P 533 0.6 0.11 871 323 < 0.10 < 0.03 > 3234 Pb 172 1.49 0.87 115 104 0.26 0.25 403 S* 162 12.5 7.72 13.0 98.2 5.00 5.09 19.6 Si 22393 28.8 0.13 779 13575 4.4 0.03 3100 Sr 113 0.5 0.41 241 68.5 0.14 0.20 495 Tl 70.4 18.98 26.96 3.7 42.7 10.10 23.67 4.2 W 37.5 < 0.10 < 0.27 > 375 22.7 < 0.10 < 0.44 > 227 Zr 2684 0.96 0.04 2810 1627 0.32 0.02 5142 B 5869 40.5 0.69 145 3558 20.4 0.57 174 Gas F 103 12.3 12.0 8.37 62.5 9.80 15.7 6.38 S 162 45.9 28.3 3.53 98.2 31.4 32.0 3.13 $ - From gravimetric analysis of filters and particulate nitric acid rinses # - Elemental feed rates calculated from target composition and test average feed rate * - Calculated from analysis of filter particulate by water dissolution and direct analysis of particulate rinse T-38 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 5.1. Results from DM100 Off-Gas Emission Samples while Processing the HLW-HMn-20 Glass Composition and Various Manganese Sources (continued). MnO2 MnCO3 11/29/2016 13:48 – 14:48 12/01/2016 13:21 – 14:21 9.21% Moisture, 100% Isokinetic 8.45% Moisture, 99.7% Isokinetic Feed# Output % Feed# Output % DF DF (mg/min) (mg/min) Emitted (mg/min) (mg/min) Emitted $ Total 68967 210 0.30 329 72996 184 0.25 396 Al 3397 5.55 0.16 612 3448 4.65 0.13 742 B 2950 16.7 0.57 176 2994 14.8 0.49 202 Bi 803 4.41 0.55 182 815 2.30 0.28 354 Ca 216 0.67 0.31 325 220 0.63 0.29 346 Cr 359 2.13 0.59 169 365 1.21 0.33 301 F* 51.8 4.83 9.33 10.7 52.6 7.91 15.0 6.65 Fe 1353 4.73 0.35 286 1373 3.7 0.27 374 K 2067 18.02 0.87 114.7 2098 14.15 0.67 148.2 La 116 < 0.10 < 0.09 > 1162 118 < 0.10 < 0.08 > 1180 Li 959 2.61 0.27 368 974 2.09 0.21 465.8 Particulate Mg 49.6 0.29 0.59 170 50.3 0.25 0.50 199 Mn 2294 5.48 0.24 418 2329 6.99 0.30 333 Na 3173 17.7 0.56 179 3221 13.7 0.43 235 Nd 56.2 < 0.10 < 0.18 > 562 57.0 < 0.10 < 0.18 > 570 Ni 311 0.20 0.07 1523 316 < 0.10 < 0.03 > 3156 P 268 < 0.10 < 0.04 > 2681 272 < 0.10 < 0.04 > 2721 Pb 86.3 0.39 0.45 221 87.6 0.32 0.37 270 S* 81.4 9.85 12.1 8.27 82.7 5.09 6.16 16.2 Si 11255 10.9 0.10 1029 11424 12.4 0.11 921 Sr 56.8 0.21 0.36 275 57.6 0.17 0.29 346.2 Tl 35.4 13.39 37.84 2.6 35.9 11.15 31.04 3.2 W 18.8 < 0.10 < 0.53 > 188 19.1 < 0.10 < 0.52 > 191 Zr 1349 0.46 0.03 2944 1369 0.38 0.03 3640 B 2950 19.4 0.66 152 2994 15.4 0.51 194 Gas F 51.8 8.59 16.6 6.03 52.6 8.77 16.7 6.00 S 81.4 25.9 31.8 3.15 82.7 27.4 33.2 3.01 $ - From gravimetric analysis of filters and particulate nitric acid rinses # - Elemental feed rates calculated from target composition and test average feed rate * - Calculated from analysis of filter particulate by water dissolution and direct analysis of particulate rinse T-39 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 5.2. Analysis of Mineral Content in Material Collected from Cyclones in the Off-gas System. XRD Analysis - Mass Removed (wt% of sample) Manganosite (MnO) – 2.2 wt% Hematite (Fe2O3) – 1.1 wt% After tests with Quartz (SiO2) – 14.8 wt% MnO 362 g Zircon (ZrSiO4) – 1.9 wt% (XBL-O-58A) Eskolite (Cr2O3) – 0.6 wt% TlCl – 0.3 wt% Pyrolucite (MnO2) – 1.4 wt% After tests with Hematite (Fe2O3) – 1.0 wt% MnO2 and Quartz (SiO2) – 9.4 wt% 490 g MnCO3 Zircon (ZrSiO4) – 1.3 wt% (XBL-O-113A) Eskolite (Cr2O3) – 0.8 wt% TlCl – 0.3 wt% T-40 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 5.3. XRF and DCP-AES Analysis of Material Collected from Cyclones in the Off-gas System After Testing (wt%). - Target XBL-O-58A XBL-O-113A Al2O3 10.88 10.73 10.77 B2O3# 16.11 24.45 24.28 Bi2O3 1.52 2.41 2.12 CaO 0.51 0.76 0.70 Cl & 0.35 0.49 Cr2O3 0.89 1.27 1.26 F$ 0.09 NM NM Fe2O3 3.28 4.98 4.60 K2O 4.22 5.62 5.76 La2O3 0.23 0.15 0.15 Li2O# 3.50 2.71 2.80 MgO 0.14 0.23 0.29 MnO 5.02 6.92 7.15 Na2O 7.25 9.53 9.25 Nd2O3 0.05 0.03 0.06 NiO 0.67 0.55 0.49 P2O5 1.04 1.45 1.36 PbO 0.16 0.26 0.23 SO3 0.34 1.36 2.04 SiO2 40.80 22.98 22.92 SrO 0.11 0.17 0.17 TiO2 & 0.05 0.04 Tl2O3 0.06 0.76 0.96 WO3 0.04 0.05 0.05 ZnO & < 0.01 0.01 ZrO2 3.09 2.23 2.06 Total 100.00 100.00 100.00 # DCP-AES analysis & Not a target constituent. T-41 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Table 5.4. Concentrations (ppmv) of Selected Species in DM100 Exhaust Measured by FTIR Spectroscopy (ppmv). Test MnO, Optimized MnO, Nominal MnO2 MnCO3 - Avg. Range Avg. Range Avg. Range Avg. Range H2O (%) 8.2 2.0 - 19.6 5.6 3.1 - 12.9 5.4 < 1.0 - 17.0 5.0 1.3 - 12.3 CO < 1.0 < 1.0 - 1.5 < 1.0 < 1.0 - 1.8 < 1.0 < 1.0 - 1.5 2.2 < 1.0 - 7.2 CO2 1905 461 - 5057 1385 817 - 4897 1292 471 - 4880 1609 714 - 5105 HCN < 1.0 NA < 1.0 NA < 1.0 NA < 1.0 NA HF 17.0 9.0 - 39.2 8.5 3.6 - 23.7 5.7 2.1 - 13.9 1.3 < 1.0 - 4.2 HCl < 1.0 < 1.0 - 3.1 < 1.0 < 1.0 - 1.2 < 1.0 < 1.0 - 1.3 < 1.0 NA NH3 < 1.0 < 1.0 - 1.4 < 1.0 NA < 1.0 < 1.0 - 1.9 1.7 < 1.0 - 4.0 HNO3 < 1.0 NA < 1.0 NA < 1.0 NA < 1.0 NA NO 28.2 < 1.0 - 90.4 18.2 5.9 - 89.6 18.2 < 1.0 - 113 6.6 2.0 - 31.5 NO2 < 1.0 < 1.0 - 1.2 < 1.0 NA < 1.0 < 1.0 - 8.9 < 1.0 < 1.0 - 1.3 HNO2 < 1.0 NA < 1.0 NA < 1.0 NA < 1.0 NA N 2O < 1.0 < 1.0 - 1.9 < 1.0 < 1.0 - 1.7 < 1.0 NA < 1.0 NA NA: Not applicable T-42 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev 1 Dilution Air Stack Pre Filter + Transition Cyclonic Fan + HEPA Line Filter Dilution Air Filter Film Cooler Feed (Simulant + Additives) Melter Figure 1.1. Schematic diagram of DuraMelter 100 vitrification system. F-1 Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev 1 Figure 1.2.a. Schematic diagram showing cross-section through the DM100-BL-melter. Plan view showing locations of lid ports. F-2 Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev 1 Figure 1.2.b. Schematic diagram showing cross-section through the DM100-BL melter. F-3 Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev 1 Figure 1.2.c. Schematic diagram showing cross-section through the DM100-BL melter. F-4 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev 1 Box Furnace Ceramic crucible 600oC half inside the local heater Dried feed (to produce ≈ 17g of glass) 1150oC Center heater at 1150oC Figure 1.3. Schematic drawing of vertical gradient furnace (VGF) for feed conversion test. F-5 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev 1 1050 1000 Bottom of crucible 950 Temperature oC 1cm above bottom 900 850 2cm above bottom 800 750 3cm above bottom 700 0 1 2 3 Distance above bottom of crucible (cm) Figure 1.4. Temperature gradient (inside the loaded ceramic crucible) of the vertical gradient furnace (VGF). F-6 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Figure 2.1. Al2O3 and MnO Concentrations in Hanford HLW. F-7 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Figure 2.2. Fe2O3 and MnO Concentrations in Hanford HLW. F-8 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Figure 2.3. Na2O and MnO Concentrations in Hanford HLW. F-9 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Cr Spectrum 1 Mn Fe Cr Mn O Cr Fe C Mn Ni Ni Al Fe Ni a) 950oC (Mn-Cr Spinel with Ni, Fe) 2 4 6 8 10 12 14 16 18 20 Full Scale 1815 cts Cursor: 20.219 (0 cts) keV Cr Mn Spectrum 1 Fe Mn Cr Cr C K Fe O Mn Si Ni Ni Al K Fe Ni b) 900oC (Mn-Cr Spinel with Ni, Fe) 2 4 6 8 10 12 14 16 18 20 Full Scale 1861 cts Cursor: 20.250 (0 cts) keV Figure 2.4. SEM images and EDS spectra of glass HLW-HMn-20 after 70 hours at a) 950oC, b) 900oC, c) 850oC and d) 800oC. F-10 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Cr Spectrum 1 Fe Mn Cr Mn O Cr Al Fe C Mn Ni Ni Fe Ni c) 850oC (Mn-Cr Spinel with Ni, Fe, Al) 2 4 6 8 10 12 14 16 18 20 Full Scale 2528 cts Cursor: 20.250 (0 cts) keV Cr Spectrum 1 Mn Fe Cr Mn O Cr C Fe Mn Al Si Ni Ni Fe Ni 0 2 4 6 8 10 12 14 16 18 20 Full Scale 1838 cts Cursor: 20.250 (0 cts) keV c) 800oC (Mn-Cr Spinel with Ni, Fe, Al) Figure 2.4. SEM images and EDS spectra of glass HLW-HMn-20 after 70 hours at a) 950oC, b) 900oC, c) 850oC and d) 800oC (continued). F-11 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 15 minutes 30 minutes 0Top View Top View Cross Section Cross Section Figure 2.5. Images of feed sample of XBL-F-19A (MnO as manganese source) after vertical gradient furnace tests (17 g glass yield). F-12 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 30 minutes 60 minutes Top View Top View Cross Section Cross Section Figure 2.6. Images of feed sample of XBL-F-79A (MnO2 as manganese source) after vertical gradient furnace tests (17 g glass yield). F-13 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 15 minutes 30 minutes Top View Top View Cross Section Cross Section Figure 2.7. Images of feed sample of XBL-F-96A (MnCO3 as manganese source) after vertical gradient furnace tests (17 g glass yield). F-14 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 With MnO With MnCO3 With MnO2 With MnO2 + Normal With MnO2 + Double Sugar Sugar HMn-10M15 HMn-10CM15 HMn-10TM15 HMn-10TSM15 HMn-10TS2M15 15 min Top View 15 min Top View 15 min Top View 15 min Top View 15 min Top View HMn-10M15 HMn-10CM15 HMn-10TM15 HMn-10TSM15 HMn-10TS2M15 15 min Cross Section 15 min Cross Section 15 min Cross Section 15 min Cross Section 15 min Cross Section Figure 2.8. Top view and cross section view of VGF samples of feeds for formulation HLW-HMn-10 with different forms of manganese and reductant. Feed samples of same manganese form and reductant are organized in one column after 15 minute and 30 minute VGF experiments. F-15 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 HMn-10M30 HMn-10CM30 HMn-10TM30 HMn-10TSM30 HMn-10TS2M30 30 min Top View 30 min Top View 30 min Top View 30 min Top View 30 min Top View HMn-10M30 HMn-10CM30 HMn-10TM30 HMn-10TSM30 HMn-10TS2M30 30 min Cross Section 30 min Cross Section 30 min Cross Section 30 min Cross Section 30 min Cross Section Figure 2.8. Top view and cross section view of VGF samples of feeds for formulation HLW-HMn-10 with different forms of manganese and reductant. Feed samples of same manganese form and reductant are organized in one column after 15 minute and 30 minute VGF experiments (continued). F-16 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 G la s s P ro d u c t io n R a t e (k g / m 2 / d a y ) 1800 1600 1400 1200 1000 800 0 20 40 60 80 100 1 hr Moving Avg. Cumulative Figure 3.1.a. Glass production rates (hourly moving averages and cumulative) for DM100 tests with the HLW-HMn-20 glass composition; MnO as the manganese source with optimized and nominal bubbling. F-17 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 G la s s P ro d u c t io n R a t e (k g / m 2 / d a y ) 1200 1000 800 600 400 200 0 20 40 60 80 100 1 hr Moving Avg. Cumulative Figure 3.1.b. Glass production rates (hourly moving averages and cumulative) for DM100 tests with the HLW-HMn-20 glass composition; MnO2 and MnCO3 as the manganese sources. F-18 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 G la s s P ro d u c t io n R a t e (k g / m 2 / d a y ) 1400 1300 1200 1100 1000 900 800 700 0 10 20 30 40 50 MnO MnO2 MnCO3 Figure 3.1.c. Cumulative glass production rates for DM100 tests with the HLW-Mn20 glass composition and various manganese sources. F-19 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 G la s s P ro d u c t io n R a t e (k g / m 2 / d a y ) 1200 1100 1000 900 800 700 600 500 0 10 20 30 40 50 MnO MnO2 MnCO3 Figure 3.1.d. Instantaneous glass production rates for DM100 tests with the HLW-Mn20 glass composition and various manganese sources. F-20 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 2000 P ro d u c t io n R a t e (k g / m 2 / d a y ) 1500 1000 500 0 Goethite Mixture MnO Hematite Fe(OH)3 MnO2 Magnetite MnCO3 Figure 3.1.e. Glass production rates for DM100 tests with the manganese- and iron-limited glass compositions and various waste loading limiting component sources. F-21 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 G la s s T e m p e ra t u re (C ) 1200 1150 1100 1050 1000 950 0 20 40 60 80 100 27" from bottom 16" from bottom 10" from bottom 5" from bottom Figure 3.2.a. Glass temperatures during DM100 tests with the HLW-HMn-20 glass composition; MnO as the manganese source with optimized and nominal bubbling. . . F-22 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 G la s s T e m p e ra t u re (C ) 1200 1150 1100 1050 1000 950 0 20 40 60 80 100 27" from bottom 16" from bottom 10" from bottom 5" from bottom Figure 3.2.b. Glass temperatures during DM100 tests with the HLW-HMn-20 glass composition; MnO2 and MnCO3 as the manganese sources. F-23 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 P le n u m T e m p e ra t u re (C ) 900 800 700 600 500 400 300 0 20 40 60 80 100 17" from top, Thermowell 17" from top, Exposed Figure 3.3.a. Plenum temperatures during DM100 tests with the HLW-HMn-20 glass composition; MnO as the manganese source with optimized and nominal bubbling. F-24 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 P le n u m T e m p e ra t u re (C ) 900 800 700 600 500 400 300 0 20 40 60 80 100 17" from top, Thermowell 17" from top, Exposed Figure 3.3.b. Plenum temperatures during DM100 tests with the HLW-HMn-20 glass composition; MnO2 and MnCO3 as the manganese sources. F-25 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 E le c t ro d e T e m p e ra t u re (C ) 1100 37 E le c t ro d e P o w e r (k W ) 1000 33 900 29 800 25 700 21 600 17 0 20 40 60 80 100 Upper Lower Bottom Power Figure 3.4.a. Electrode temperatures and power during DM100 tests with the HLW-HMn-20 glass composition; MnO as the manganese source with optimized and nominal bubbling. . . F-26 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 E le c t ro d e T e m p e ra t u re (C ) 1100 28 E le c t ro d e P o w e r (k W ) 1000 24 900 20 800 16 700 12 600 8 0 20 40 60 80 100 Upper Lower Bottom Power Figure 3.4.b. Electrode temperatures and power during DM100 tests with the HLW-HMn-20 glass composition; MnO2 and MnCO3 as the manganese sources. F-27 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 M e lt P o o l R e s is t a n c e (O h m s ) 0.16 29 E le c t ro d e P o w e r (k W ) 0.13 26 0.1 23 0.07 20 0.04 17 0 20 40 60 80 100 Resistance Power Figure 3.5.a. Melt pool resistance and total electrode power during DM100 tests with the HLW-HMn-20 glass composition; MnO as the manganese source with optimized and nominal bubbling. F-28 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 M e lt P o o l R e s is t a n c e (O h m s ) 0.12 24 E le c t ro d e P o w e r (k W ) 0.1 21 0.08 18 0.06 15 0.04 12 0 20 40 60 80 100 Resistance Power Figure 3.5.b. Melt pool resistance and total electrode power during DM100 tests with the HLW-HMn-20 glass composition; MnO2 and MnCO3 as the manganese sources. F-29 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 18 G la s s P o o l B u b b lin g (lp m ) 16 14 12 10 8 6 4 2 0 0 20 40 60 80 100 Figure 3.6.a. Melt pool bubbling during DM100 tests with the HLW-HMn-20 glass composition; MnO as the manganese source with optimized and nominal bubbling. . F-30 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 10 G la s s P o o l B u b b lin g (lp m ) 8 6 4 2 0 0 20 40 60 80 100 Figure 3.6.b. Melt pool bubbling during DM100 tests with the HLW-HMn-20 glass composition; MnO2 and MnCO3 as the manganese sources. F-31 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 6 5 4 wt % 3 2 1 0 0 100 200 300 400 500 600 700 800 900 Target Bi2O3 Target MnO Target PbO Measured Bi2O3 Measured MnO Measured PbO Figure 4.1.a. DM100 product and target glass compositions determined by XRF. F-32 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 45 40 35 30 25 wt % 20 15 10 5 0 0 100 200 300 400 500 600 700 800 900 Target Al2O3 Target Na2O Target SiO2 Measured Al2O3 Measured Na2O Measured SiO2 Figure 4.1.b. DM100 product and target glass compositions determined by XRF. F-33 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 7 6 5 4 wt % 3 2 1 0 0 100 200 300 400 500 600 700 800 900 Target CaO Target Fe2O3 Target MgO Measured CaO Measured Fe2O3 Measured MgO Figure 4.1.c. DM100 product and target glass compositions determined by XRF. F-34 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 4.5 4 3.5 3 2.5 wt % 2 1.5 1 0.5 0 0 100 200 300 400 500 600 700 800 900 Target Cr2O3 Target K2O Target SO3 Measured Cr2O3 Measured K2O Measured SO3 Figure 4.1.d. DM100 product and target glass compositions determined by XRF. F-35 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 7 6 5 4 wt % 3 2 1 0 0 100 200 300 400 500 600 700 800 900 Target NiO Target P2O5 Target ZrO2 Measured NiO Measured P2O5 Measured ZrO2 Figure 4.1.e. DM100 product and target glass compositions determined by XRF. F-36 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 0.25 0.2 0.15 wt % 0.1 0.05 0 0 100 200 300 400 500 600 700 800 900 Target La2O3 Target Nd2O3 Measured La2O3 Measured Nd2O3 Figure 4.1.f. DM100 product and target glass compositions determined by XRF. F-37 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 0.14 0.12 0.1 0.08 wt % 0.06 0.04 0.02 0 0 100 200 300 400 500 600 700 800 900 Target SrO Target Tl2O Measured SrO Measured Tl2O3 Figure 4.1.g. DM100 product and target glass compositions determined by XRF. F-38 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 Mn Cr Spectrum 1 Fe Cr O Mn Cr Fe Mn C Ni Ni Al Fe Ni 0 2 4 6 8 10 12 14 16 18 20 Full Scale 3562 cts Cursor: 20.250 (0 cts) keV a. Fe Mn Spectrum 1 Mn Fe Cr Cr Mn O Cr C Ni Ni Zn Al Fe Ni Cd Cd Zn Zn 0 2 4 6 8 10 12 14 16 18 20 Full Scale 2142 cts Cursor: 20.250 (0 cts) keV b. Figure 4.2. SEM images and EDS spectra of a) XBL-G-58A discharged after MnO tests b) XBL-G-89C discharged after MnO2 test. F-39 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 120 100 80 NO (ppmv) 60 40 20 0 0 5 10 15 20 25 30 35 40 45 50 55 MnO, Optimized MnO, Nominal MnO2 MnCO3 Figure 5.1.a. FTIR monitored NO emissions while processing the HLW-HMn-20 glass composition. F-40 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 6000 5000 4000 CO2 (ppmv) 3000 2000 1000 0 0 5 10 15 20 25 30 35 40 45 50 55 MnO, Optimized MnO, Nominal MnO2 MnCO3 Figure 5.1.b. FTIR monitored CO2 emissions while processing the HLW-HMn-20 glass composition. F-41 The Catholic University of America High Waste Loading Glass Formulation Development for High-Mn HLW Vitreous State Laboratory Final Report, VSL-17R4120-1, Rev. 1 20 18 16 14 12 H2O (%) 10 8 6 4 2 0 0 5 10 15 20 25 30 35 40 45 50 55 MnO, Optimized MnO, Nominal MnO2 MnCO3 Figure 5.1.c. FTIR monitored water content of exhaust while processing the HLW-HMn-20 glass composition. F-42