Ternary Liquid-Crystalline Mixture Showing Broad Antiferroelectric Smectic CA* and Glassy Hexatic Smectic XA* Phases Aleksandra Deptuch, Anna Drzewicz, Marcin Piwowarczyk, Michał Czerwiński, Mateusz Filipow, Mateusz Pączek, Ewa Juszyńska-Gałązka Abstract A ternary liquid crystalline mixture was designed to obtain a tilted hexatic smectic phase in the glassy state. Structural, electro-optic, and dielectric properties of the mixture are investigated, and selected measurements are also performed for its pure components. In particular, the electron density profile perpendicular to smectic layers is determined from the X-ray diffraction data and compared to the results of density functional theory calculations both for the mixture and pure components. Comparison of the experimental smectic layer spacing and tilt angle in the mixture allows us to assess whether molecular dimerization is likely to occur. On the mesoscopic scale, the helical pitch is determined in the SmCA* phase of the mixture, and selective reflection of light is observed under a polarizing microscope in the SmC*, SmCA*, and SmXA* phases. The glass transition in the SmXA* phase is observed in calorimetric results. At the same time, the dielectric spectra do not directly reveal the primary α-process, although the secondary β- and γ-processes are detected. Overall, the results show that the ternary mixture stabilizes a broad SmCA* phase and enables vitrification of the hexatic SmXA* phase, while the structural data suggest a change in the molecular organization between the SmC* and SmCA* phases. [jp6c02873_0016.webp] [jp6c02873_0014.webp] Introduction The glass transition, or vitrification, is associated with a strong slowdown of molecular relaxation, which prevents thermodynamic equilibration, including crystallization. This enables the preservation of, e.g., desired optical properties or charge mobility of a less-ordered phase in a given material below the glass transition temperature. , The glass transition can occur for materials which have any kind of positional, orientational, or conformational disorder, starting from an isotropic liquid or an amorphous polymer, − via various liquid-crystalline phases − to orientationally disordered (ODIC) and conformationally disordered (CONDIS) crystal phases. In this work, we focus on smectic phases, i.e., lamellar liquid-crystalline phases formed by elongated molecules, with molecular tilt with respect to the smectic layer normal given by the magnitude Θ and phase φ. The smectic phases formed by chiral molecules include, in order of decreasing temperature: − smectic A* (SmA*) – random φ and average tilt angle equal to zero; SmCα* – φ twisting helically from layer to layer with a short pitch (∼ a few smectic layers); SmC* – approximately constant φ in neighboring layers, twisting helically with a long pitch (∼ hundreds of smectic layers); SmCF2* – φ twisting with a period of four layers; SmCF1* – φ twisting with a period of three layers; SmCA* – φ changing by approximately 180° from layer to layer, twisting helically with a long pitch (∼ hundreds of smectic layers). The magnitude Θ is nonzero in SmC* and all its variants; it can be also nonzero in SmA* (de Vries phase). In all listed smectic phases, the ordering of molecules within smectic layers is short-range (liquid-like). On decreasing temperature, the SmA*, SmC*, and SmCA* phases may transform into their hexatic equivalents, where intralayer domains with a local hexagonal order are larger than in SmA*, SmC*, and SmCA*, and they are oriented in the same direction. SmBhex* is a hexatic counterpart of SmA*. For the tilted SmC* phase, the hexatic version is either SmF* or SmI* with different orientations of hexagonal domains with respect to the tilt phase φ (and similarly SmFA* or SmIA* for SmCA*). − SmF* (SmFA*) and SmI* (SmIA*) can generally be distinguished only by X-ray diffraction on an oriented sample. The notation SmX* (or SmXA* for the antiferroelectric analogue) is used throughout this paper. The chiral tilted smectic phases have potential applications in liquid crystal displays thanks to their ability of bistable or tristable switching under an electric field , and for the selective reflection of light (SRL) thanks to a helical ordering. , The recent results on (S)-4′-(1-methylheptyloxycarbonyl)­biphenyl-4-yl 4-[5-(2,2,3,3,4,4,4-heptafluorobutoxy)­pentyl-1-oxy]-2-fluorobenzoate indicate that the helix pitch in the glassy SmCA* phase is rather constant, which opens the possibility of applications in optical filters, although the glass transition temperature of this compound is low, ca. 230 K. The transition to a hexatic phase is reported to change the helix pitch: refs , mention a decrease in the helix pitch and results from ref indicate an increase in the helix pitch in the hexatic phase. Despite extensive studies on chiral smectic phases, the helical order in the SmXA* phase has received limited attention, especially in the glassy state. This study focuses on the ternary mixture of (S)-4-[(1-methylheptyloxy)­carbonyl]­phenyl 4′-octyloxy-4-biphenylcarboxylate (MHPOBC), (S)-4′-(1-methylheptylcarbonyl)­biphenyl-4-yl 4-[2-(2,2,3,3,4,4,4-heptafluorobutoxy)­etyl-1-oxy]­benzoate (3F2HPhH6), and (S)-4′-(1-methylheptylcarbonyl)­biphenyl-4-yl 4-[3-(2,2,3,3,4,4,4-heptafluorobutoxy)­propyl-1-oxy]­benzoate (3F3HPhH6), with an MHPOBC:3F2HPhH6:3F3HPhH6 molar ratio of 0.5:0.25:0.25. The mixture is further denoted as MIX23HH6. The molecular formulas of the MIX23HH6 components are presented in . MHPOBC has the phase sequence Cr (357 K), SmCA* (391 K) SmCFI1* (392 K) SmC* (394 K) SmCα* (395 K) SmA* (422 K) Iso on heating (the exact narrow temperature ranges of SmCFI1*, SmC*, and SmCα* phases vary slightly between sources). , Additionally, a monotropic SmXA* phase is formed at 338 K on the cooling run only. , The glass transition of SmXA* in MHPOBC is not observed at cooling rates up to 40 K/min. The phase sequence of 3F2HPhH6 on heating is Cr (342 K) SmCA* (388 K) SmC* (401 K) Iso and that of 3F3HPhH6 is Cr (352 K) SmCA* (389 K) Iso. The presence of monotropic phases and glass-forming properties of these two compounds has not been investigated yet, but the results for longer 3FmHPhH6 homologs with m = 4, 5, 7 indicate that the hexatic SmXA* phase may be present on supercooling. , Therefore, the formation of SmXA* in the mixture can be expected. The main aims of this work are to check the presence of SRL in the smectic phases, particularly the hexatic phase and its glassy state, and to compare the structures of smectic phases in the mixture with those in the pure components. In the first part, the behavior of supercooled pure 3F2HPhH6 and 3F3HPhH6 components is investigated together with the MIX23HH6 mixture by differential scanning calorimetry (DSC) and polarized optical microscopy (POM) methods at selected cooling/heating rates. In the second part, the structure of the smectic phases of MIX23HH6 and its components is investigated by X-ray diffraction (XRD). The smectic layer spacing is determined from the positions of low-angle diffraction peaks, and the electron density distribution perpendicular to the smectic layers is obtained from the integrated intensities of these peaks. In the third part, the dielectric strength and relaxation times in 3F2HPhH6, 3F3HPhH6, and MIX23HH6 are determined by broadband dielectric spectroscopy (BDS). The corresponding results for MHPOBC were reported elsewhere; therefore, only extended XRD data for this component are presented (the results in ref did not include the electron density profile). The fourth and fifth parts focus exclusively on MIX23HH6. They cover SRL originating from the helical order as well as their electrical, electro-optical, and switching behavior in an electric field (specifically spontaneous polarization, tilt angle, and switching time). Experimental and Computational Details The (S)-4-[(1-methylheptyloxy)­carbonyl]­phenyl 4′-octyloxy-4-biphenylcarboxylate (MHPOBC), (S)-4′-(1-methylheptylcarbonyl)­biphenyl-4-yl 4-[2-(2,2,3,3,4,4,4-heptafluorobutoxy)­etyl-1-oxy]­benzoate (3F2HPhH6), and (S)-4′-(1-methylheptylcarbonyl)­biphenyl-4-yl 4-[3-(2,2,3,3,4,4,4-heptafluorobutoxy)­propyl-1-oxy]­benzoate (3F3HPhH6) were synthesized at the Institute of Chemistry of the Military University of Technology in Warsaw according to synthetic routes described in ref (MHPOBC) and refs , (3F2HPhH6, 3F3HPhH6). The ternary mixture MIX23HH6 of MHPOBC:3F2HPhH6:3F3HPhH6 with the molar ratio 0.5004(4):0.2491(3):0.2505(3) was prepared by dissolution of pure compounds in acetone. After the evaporation of acetone, the mixture was heated to 433 K to reach the isotropic liquid phase and cooled down to room temperature. The DSC measurements were performed under a nitrogen atmosphere for the 3F2HPhH6, 3F3HPhH6, and MIX23HH6 samples weighing 6.69, 8.41, and 5.75 mg, respectively, and were contained within aluminum pans. The DSC scans were collected with a DSC 2500 (TA Instruments) calorimeter at 2, 5, 10, 15, 20, 25, 30, 35, and 40 K/min cooling/heating rates in the temperature range between 173 and 433 K. First, each sample was heated to 433 K at 10 K/min (1st heating), and then, the measurements for each rate were performed during the cooling-heating cycle. The DSC results were analyzed with TRIOS software. The POM observations in the transmission mode were performed on the 3F2HPhH6, 3F3HPhH6, and MIX23HH6 films placed between two thin glass slides without any alignment layers. The cooling/heating rate was 10 K/min for all samples, and additionally 40 K/min for 3F2HPhH6 and 1 K/min for 3F3HPhH6. The observations in the reflection mode were conducted for MIX23HH6 in an electro-optic cell with a 5 μm thickness, providing a homeotropic alignment. The POM textures were captured using a Leica DM2700 P polarizing microscope and a Linkam temperature stage. The weighted average intensity of each image was calculated using TOApy, while red, green, and blue channel components were determined using ImageJ. The XRD measurements were performed on the MHPOBC, 3F2HPhH6, 3F3HPhH6, and MIX23HH6 flat samples in a sample holder of dimensions 13 mm × 10 mm × 0.2 mm. The XRD patterns were collected with an X’Pert PRO (PANalytical) diffractometer in Bragg-Brentano geometry, using CuKα radiation (λ CuKα1 = 1.540562 Å, λ CuKα2 = 1.544390 Å), during cooling from 433 to 298 K. Calibration of the 2θ position was done using the NIST Standard Reference Material 675, supplied by Merck. To compensate for small changes in the sample height after the first heating run, the additional systematic shift in the 2θ angle was corrected based on the positions of the 2nd, 3rd, and 4th diffraction peaks deep in the SmCA* or SmXA* phase. The XRD patterns were analyzed using WinPLOTR and OriginPro. The BDS measurements were carried out on the 3F2HPhH6, 3F3HPhH6, and MIX23HH6 samples of ca. 50 μm thickness placed between gold electrodes with polytetrafluoroethylene spacers. The BDS spectra were collected with a Novocontrol impedance analyzer for frequencies between 0.1 Hz and 10 MHz during cooling from the isotropic liquid to 173 K and then during heating back to the isotropic liquid. The BDS spectra were analyzed using OriginPro. The UV–Vis–NIR spectroscopic measurements were performed on the MIX23HH6 sample in homeotropic alignment with a Shimadzu spectrometer in the range of 360–3000 nm. The helix pitch was determined as p h = λmin/1.5, , where λmin is the wavelength at the SRL maximum. The electric field switching studies were performed for the MIX23HH6 sample in a surface-stabilized bookshelf geometry using a special driving scheme for the SmCA* phase. The setup comprised the R&S HMF2550 function generator, the FLC F20AD amplifier, and a Biolar PI, PZO Poland, polarizing microscope with a Linkam THMS 600 temperature stage. The spontaneous polarization and tilt angle were determined by the reversal current method with the R&S HM0724 oscilloscope and by observation of the Clark–Lagerwall effect with the Thorlabs PDA100A photodetector, respectively. The DFT geometry optimizations for isolated molecules were carried out in Gaussian 16, Revision C.01 (B3LYP-D3­(BJ) exchange-correlation functional, − 6-31+Gd basis set). The molecules were visualized in Avogadro. The starting model for MHPOBC was based on the experimental molecular conformation in a crystal phase , and tilt angle. The starting models for 3F2HPhH6 and 3F3HPhH6 were based on a strongly twisted conformation inferred previously for 3F7HPhH6, which belongs to the same homologous series with an identical fluorinated chain and chiral center, contributing to the molecular shape. Results and Discussion Phase Sequence The DSC thermograms of each sample are presented in . The phase transition temperatures were determined as the onset temperatures. An exception was the pair of overlapping anomalies observed for 3F3HPhH6 at 2 K/min, where the peak temperature of the second anomaly was used. The glass transition temperature was assumed to be at the half-height of the step-like anomaly. The results are presented in as a function of the cooling/heating rate. Phase transition temperatures and corresponding enthalpy changes are presented in . Complementary POM data are provided in Figures S1–S10 of the Supporting Information Materials. Two smectic phases are observed for 3F2HPhH6 by DSC (a, a) and POM (Figures S1–S4) above the melting temperature, in agreement with SmC* and SmCA* reported in ref . 3F2HPhH6 crystallizes on cooling at all applied cooling rates. During fast cooling at 25–40 K/min, there is a distortion of the exothermic anomaly related to crystallization. Four scenarios may account for this distortion: (1) two-step crystallization, (2) crystallization followed by the glass transition of the remaining SmCA* fraction, (3) SmCA* → SmXA* transition followed by crystallization, (4) SmCA* → SmXA* transition followed by the glass transition of SmXA*. The POM textures collected during cooling at 40 K/min (Figure S3) indicate scenario (3). The abrupt change of textures’ color from pink to green, with a peak in the green component observed at 297 K, is interpreted as the SmCA* → SmXA* transition. The next change in color from green to red is attributed to incomplete crystallization, where numerous small crystallites do not distort the fan-shaped texture. During heating at 15–40 K/min, a broad exothermic anomaly with an onset at 292–305 K is observed in DSC thermograms below the melting temperature of a crystal phase, corresponding to the cold crystallization of the smectic phase supercooled in the prior fast cooling run. The POM observations at the 40 K/min heating rate (Figure S4) confirm cold crystallization; the texture changes gradually in the 300–320 K range from the red fan-shaped one to the brown texture of a crystal phase observed during slower cooling/heating at 10 K/min (Figures S1 and S2). DSC results at 5–40 K/min (b, b) and POM observations at 10 K/min (Figures S5 and S6) indicate one smectic phase of 3F3HPhH6, which corresponds to SmCA* reported in ref However, DSC results at 2 K/min show the splitting of the anomaly at ∼390 K, which suggests an additional smectic phase between SmCA* and the isotropic liquid (inset in b). On the other hand, POM textures collected at a low 1 K/min rate do not reveal any additional smectic phase (Figures S7 and S8). 3F3HPhH6 crystallizes at all applied cooling rates. During heating, the broad anomaly related to cold crystallization is observed below the melting temperature, but the corresponding enthalpy change is very small, about 1 kJ/mol in total, which means that crystallization is almost complete in the cooling run. We propose that supercooled SmCA*, present in a small fraction below the melt crystallization temperature, undergoes a transition to SmXA*; it corresponds to a small anomaly observed at 290–300 K during cooling. The MIX23HH6 mixture shows four smectic phases, detected both by DSC (c, c) and POM (Figures S9 and S10): enantiotropic SmA*, SmC*, SmCA*, and monotropic, metastable hexatic SmXA*, which is present below the melting temperature. SmXA* undergoes a glass transition at T g = 265.5 K on cooling and 273.4 K on heating. Melt crystallization is not observed on cooling, while cold crystallization occurs on heating above T g , with an onset at 304–305 K. The crystal phase melts at 313–320 K and the melting enthalpy decreases from ∼10 K/min at 2 K/min to only ∼1 kJ/mol at 40 K/min. This explains why the POM texture in the region of cold crystallization observed at 10 K/min (Figure S10, 308 K) is a fan-shaped texture of a smectic phase: cold crystallization is incomplete, and the formed crystallites are small. The isoconversional method was used to determine the effective activation energy E eff for the crystallization of pure 3F2HPhH6 (Figure S11) and 3F3HPhH6 (Figure S12). The activation plot in this method is based on the logarithm of the conversion rate: dx/dt, at a selected conversion degree x, plotted against the temperature Tx corresponding to the selected x value: − where f(x) and A are fitting parameters. The dx/dt and Tx values were determined from DSC thermograms in the region of melt crystallization at different cooling rates: 2–20 K/min for 3F2HPhH6 and 2–40 K/min for 3F3HPhH6. The high cooling rates were excluded from analysis for 3F2HPhH6 because of the SmCA* → SmXA* transition overlapping with crystallization. The E eff values are obtained as a function of x, but they can be plotted approximately as a function of temperature by taking middle Tx from each linear part of the In­(dx/dt) vs 1000/T x plot. , Positive E eff indicates that crystallization occurs in a temperature region of high nucleation rate and low diffusion (crystal growth) rate, thus, the overall crystallization kinetics is constrained by diffusion. Negative E eff describes a reverse situationcrystallization occurs in a temperature region of low nucleation rate and high diffusion rate, and the constrain on the overall crystallization is imposed by nucleation. , Typically, positive E eff is obtained at lower temperatures and negative E eff at higher temperatures; E eff ≈ 0 characterizes the temperature region of the fastest crystallization. 3F2HPhH6 has two regions of E eff ≈ 0: at 298–299 K and around 311 K (Figure S11c). At intermediate temperatures, E eff < 0, which means nucleation-constrained crystallization. Crystallization of 3F3HPhH6 is the fastest around 307 K and strongly nucleation-constrained around 310 K (Figure S12c). The temperature region of melt crystallization is narrower for 3F3HPhH6 than for 3F2HPhH6. Structure of Smectic Phases The X-ray diffraction patterns of 3F2HPhH6, 3F3HPhH6, and MHPOBC show that all pure components crystallize on slow cooling (a). In contrast, MIX23HH6 does not show crystallization on slow cooling down to room temperature (b). The low-angle peaks with Miller indices (00l), indicated for MIX23HH6 in b, are related to the positional layer order. The layer spacing d is determined from the Bragg equation lλCuKα1 = 2d sin θ00l , , where θ00l is the low-angle (00l) peak position and l is an integer (c). MHPOBC shows a layer shrinkage of 3.4% between SmA* and SmCA* and a 6.5% increase in the layer spacing between SmCA* and SmXA*. The layer shrinkage in 3F2HPhH6 and 3F3HPhH6 is small, only 2.4% and 1.9%, respectively. The layer spacing of 3F3HPhH6 increases weakly just below the Iso → SmCA* transition, from 29.6 Å at 392 K to 29.7 Å at 393 K, which corresponds to a double transition observed in DSC thermograms. The layer shrinkage in MIX23HH6 between SmA* and SmCA* is 8.9% and the increase in the layer spacing between SmCA* and SmXA* is 4.0%. Intensities of (00l) peaks are related to the distribution of electron density ρ­(z) in the direction perpendicular to the smectic layers. ,, Molecules in smectic phases rotate around their short axes. Consequently, ρ­(z) is centrosymmetric with respect to the middle of a smectic layer and is described by a series of cosines: Structure factors F 00l are related to the integrated intensities of (00l) peaks as |F00l|=I00l/Lp , where the Lorentz-polarization correction for an aligned sample is calculated as Intensities of (00l) peaks from smectic layers are much stronger than the diffuse maximum at higher 2θ angles (originating from an intralayer order) in the XRD patterns of MIX23HH6 and its components. This indicates a mainly homeotropic alignment of the samples, and for the Lp correction can be applied in this case. The absolute values of F 00l obtained from experimental intensities are presented in . The largest structure factor for 3F2HPhH6 is |F 003|, which means that the ρ­(z) distribution is mainly described by the cos­(6πz/d) component. For 3F3HPhH6, MHPOBC, and MIX23HH6, the largest structure factor is |F 001|, so the main component of ρ­(z) is cos­(2πz/d). The signs of F 00l are unknown, but the negative (−) sign of the main F 00l factor (F 001 or F 003) can be inferred when one assumes that ρ­(z) has local minima between smectic layers (z = 0 and z = d) and local maximum around the middle of a smectic layer (z = d/2). The signs of minor F 00l are more arbitrary because they affect total ρ­(z) to a smaller extent. After testing various signs of F 00l and comparing with results of DFT calculations (discussed later), the final set used to calculate ρ­(z) from is −|F 00 l | for all l, except +|F 005| in MIX23HH6 (). The electron density profiles of 3F2HPhH6 (a) and 3F3HPhH6 (b) have local maxima not only around the middle of smectic layers, related to the aromatic core, but also close to the borders of smectic layers, related to the fluorinated chain. These side maxima are particularly strong for 3F2HPhH6, probably because of a closer proximity of the fluorinated chain and the oxygen atoms adjacent to the aromatic ring than in 3F3HPhH6 (). The side maxima in ρ­(z) are absent in MHPOBC (c). The electron density profile in MIX23HH6 resembles that of MHPOBC at higher temperatures, while the side maxima in ρ­(z) arise upon approaching the SmCA* → SmXA* transition (d). The ρ­(z) profiles were predicted based on DFT calculations. This is not straightforward, as considered compounds have flexible molecules. To reproduce it to some extent, four conformations of similar length and shape were optimized for each compound. The molecular models were properly oriented, so that the z-axis corresponded to the smectic layer normal. The centrosymmetric ρ­(z) profiles were obtained by flipping the calculated electron density along the center of a smectic layer and averaging with its mirror image. Then they were smoothed by fitting (Figures S13–S15, see also ref ). Results vary between conformations; therefore, ρ­(z) profiles averaged over conformations were calculated (). The DFT results for 3F2HPhH6 and 3F3HPhH6 (a,b), although do not reproduce quantitatively relative magnitudes of |F 00 l |, show distinct lateral maxima in qualitative agreement with experimental ρ­(z) profiles (a,b). It is different for MHPOBC, where the DFT results predict strong lateral maxima in ρ­(z) (c), which are absent or weak in the experimental ρ­(z) (c). This can be explained by the low smectic order parameters τ l for l > 1 in MHPOBC, as obtained in ref (τ1 ≈ 0.8, τ2 ≈ 0.35, and τ3 < 0.1), which lower the corresponding intensities of (00l) peaks. Dielectric Relaxation Processes Representative BDS spectra in the smectic phases are shown for MIX23HH6 in . The weak soft mode (SM) and strong Goldstone mode (GM) , are observed in the SmA* phase of MIX23HH6 and the SmC* phase of 3F3HPhH6 and MIX23HH6, respectively. The low-frequency PL phason and high-frequency PH phasons , are observed in the SmCA* phase of all samples. There is an additional Maxwell–Wagner–Sillars (MWS) process at low frequencies in the SmC* phase of MIX23HH6 and SmCA* phase of 3F3HPhH6 and MIX23HH6. In the hexatic SmXA* phase of MIX23HH6, a new Phex phason appears on the low-frequency side of PH. The α-relaxation expected for glass-forming materials ,,, is not explicitly visible for MIX23HH6. Finally, in the SmXA* glass of MIX23HH6, the weak secondary β-relaxation and γ-relaxation are observed. There are also weak relaxation processes in the crystal phases of 3F2HPhH6 and 3F3HPhH6, denoted as cr-I, cr-II, cr-III, and cr-IV in the order of increasing frequency (). The cr-II process is observed for both compounds, cr-I and cr-IV only for 3F2HPhH6 and cr-III only for 3F3HPhH6. The relaxation times τ were determined by fitting to BDS spectra the complex function describing the dielectric permittivity ε* based on the Havriliak–Negami (HN) model: ,, where ε∞ is the real part of ε* at the frequency limit f → ∞, Δε is the dielectric strength, τ HN is the HN relaxation time, a and b are shape parameters, S 1, n 1 and S 2, n 2 describe the low-frequency background. If b = 1, the HN model simplifies to Cole–Cole (CC) model and τ HN = τ, corresponding to the peak in ε′′. If b ≠ 1, τ HN does not correspond to the peak in ε′′. The relaxation time τ is then calculated using the formula: Relaxation processes were fitted mainly by the CC model, except the β-process fitted by the HN model. The activation plots of τ are presented in . Most of the relaxation processes show an Arrhenius dependence of the relaxation time on temperature, τ­(T) = τ0 exp­(ΔE/k B T), where τ0 is the pre-exponential constant, ΔE is the activation energy, and k B is the Boltzmann constant. The PL process has ΔE = 119.6(6), 119.7(9), and 109.7(7) kJ/mol for 3F2HPhH6, 3F3HPhH6, and MIX23HH6, respectively. The Arrhenius behavior and high ΔE of PL correspond to overlapping with the s-process, related to rotations around short molecular axes. The MWS process has ΔE = 67.3(9) and 68(2) kJ/mol in 3F3HPhH6 and MIX23HH6, respectively. The PH and Phex processes in the SmXA* phase of MIX23HH6 are characterized by ΔE = 301(4) kJ/mol for PH and 341(5) kJ/mol for Phex. Such large ΔE values are caused likely by approaching the glass transition. The β-process in MIX23HH6 has ΔE = 77.0(4) and 22(2) kJ/mol above and below 288 K. The latter value can be interpreted, according to earlier DFT calculations for a very similar molecule, as conformational changes within one of the terminal chains. The former, higher value includes probably also rotation of the benzene ring. The cr-I process has ΔE = 68.1(4) kJ/mol. Similar ΔE values are obtained for cr-II: 60.7(2) kJ/mol for 3F2HPhH6 and 60.3(2) kJ/mol for 3F3HPhH6. The cr-III process shows two ΔE values, 52.5(3) and 29(1) kJ/mol, above and below 190 K, which may be caused by the transition between two crystal phases. Finally, cr-IV has ΔE = 30.5(2) kJ/mol. The energy barriers of processes in the crystal phases of 3F2HPhH6 and 3F3HPhH6 indicate their origin in intramolecular rotations. The energy barrier of 50–60 kJ/mol corresponds to rotation of the benzene ring and that of 30 kJ/mol corresponds to rotation of the chiral chain, according to DFT calculations. It means that the crystal phases of 3F2HPhH6 and 3F3HPhH6 are CONDIS phases. The γ-relaxation time in MIX23HH6 cannot be fitted reliably with the Arrhenius formula as its activation plot is almost horizontal, indicating a very low ΔE. The PH process in SmCA* shows a super-Arrhenius behavior described by an empirical Vogel–Fulcher–Tammann (VFT) equation, τ­(T) = τ0exp­(B/(T – T V )), where B is a constant with units of temperature and T V is the Vogel temperature. The VFT formula is usually applied for fitting of the α-relaxation time and the glass transition temperature T g is defined at τ = 100 s. However, if the α-relaxation time cannot be measured, extrapolation of the PH-relaxation time to 100 s enables determination of a slightly overestimated T g . The expected glass transition temperatures obtained from fitting the VFT formula to the PH-relaxation time in SmCA* are 268(1), 284(2), and 276.1(2) K for 3F2HPhH6, 3F3HPhH6, and MIX23HH6, respectively. The PH-relaxation time in the SmXA* phase of MIX23HH6 changes its temperature dependence to an Arrhenius behavior, and extrapolation to 100 s gives T g = 268(3) K. Both T g values obtained from the BDS spectra of MIX23HH6 are close to calorimetric T g = 265–273 K. The absence of the α-relaxation can be explained by its initial overlapping with the β-relaxation and rapid shifting out of the frequency range at T g , which is rather high compared to T g = 230–247 K for pure compounds forming the SmXA* glass, where the α-process was observed. ,, Helical Order in MIX23HH6 The UV–Vis–NIR spectroscopy measurements in SmCA* show a decrease of the helix pitch p on cooling, with SRL in the visible range from 326 K down to the SmCA*/SmXA* transition at 308 K (). The helix inversion temperature, estimated by linear extrapolation of 1/p to zero, is equal to 356.4(9) K. Another method to observe the helix inversion is POM in the reflection mode, where it shows as a maximum in the intensity of all rgb components (Figures S16, S17). The inversion temperature obtained by POM is 360 K on cooling, slightly higher than that from spectroscopic results. There is a hysteresis of 19–25 K in the thermochromic effect: maxima of rgb components occur at 318, 314, and 310 K on cooling and at 343, 333, and 330 K on heating. This shift explains why the inversion is not observed on heating as it would occur above the transition temperature to SmC*. The POM observations reveal SRL in SmC* of blue light on cooling and of blue and green light on heating (Figures S18, S19). The SRL deep in SmXA* is out of the range of a spectrometer, but POM observations show a dark blue image (280 K in Figure S16). This may be a sign of a rather short helix (p < 200 nm) in SmXA*. Interestingly, below 260 K there is a color change to dark brown (200 K in Figure S16), which suggests that it has some relationship to the glass transition. However, the exact mechanism for this color change is unknown. Electro-Optical Response and Switching Behavior of MIX23HH6 in an External Electric Field The switching time τ sw in SmCA* increases on cooling from 33 μs at 387 K to 146 μs at 348 K. On further cooling, τ sw increases more rapidly up to 393 μs at 308 K (a). The spontaneous polarization P s has a maximum value of 258 nC/cm2 at 308 K and changes with temperature both in SmC* and SmCA* according to the formula P s (t) = P 0(T c – T) p , where P 0 = 24(4) nC/cm2, T c = 401(1) K, p = 0.50(4) (b). The tilt angle Θ increases on cooling and reaches 38° close to the SmCA*/SmXA* transition temperature. The nonzero Θ values of 5–7.5° in SmA* are caused by the electroclinic effect (c). The tilt angle follows the power function Θ­(t) = Θ0(T c – T) p , where Θ0 = 22.1(6)°, T c = 401.5(2) K, and p = 0.13(1). The difference in p values for P s and Θ means that these order parameters are not proportional to each other, which can be observed for large tilt angles, where higher-order terms have to be included in the free-energy expansion. Moreover, molecules of MIX23HH6 components can take strongly nonlinear shapes, giving a significant contribution to the measured optical tilt angle, even if the steric tilt angle of the molecules is low. The smectic layer spacing depends on the tilt angle as d(Θ) = L acos­(Θ – δΘ), where L is the molecular length and δΘ is a shape parameter, describing the deviation of a molecule from a rod-like shape. The experimental d and Θ values were compared on a scale of the reduced temperature T – T c , where T c corresponds to the SmA* → SmC* transition, which occurs at a slightly higher temperature in electro-optic measurements than in XRD. The fitting results for MIX23HH6 are L = 32.31(2) Å, δΘ = 16.7(2)° in SmC* and L = 31.19(5) Å, δΘ = 25.2(5)° in SmCA* (d). For comparison, mean L and δΘ values obtained by DFT for 3F2HPhH6, 3F3HPhH6, and MHPOBC are 29, 30, and 32.5 Å and 28°, 25°, and 23.5°, respectively. The L value includes the nonbonded distance between terminal atoms: 3.22 Å for C,F and 3.59 Å for C,C. The weighted average of calculated L and δΘ, based on the composition of MIX23HH6, is 31 Å and 25°. The L value is slightly larger and δΘ angle is much lower in SmC*, which can be caused by dimerization of some MHPOBC molecules in the mixture. By dimer we understand two molecules connected by electrostatic interactions, which consequently form one structural unit. , The smectic layer spacing of 3F2HPhH6 and 3F3HPhH6 is smaller than the average molecular lengths, which does not suggest dimer formation. However, dimerization occurs very likely in pure MHPOBC, as the smectic layer spacing >34 Å is larger than the length of a single molecule, and it was taken into account while calculating ρ­(z) in c. Meanwhile, the very good agreement between calculated and experimental L and δΘ values below the SmC* → SmCA* transition suggests that MHPOBC dimers are absent, or at least much less important, in the SmCA* phase of MIX23HH6. This result was applied to predict the ρ­(z) profile in MIX23HH6 from DFT calculations. The same molecular models as in and Figures S13–S15 were used, only tilted to match the experimental tilt angle in MIX23HH6 deep in SmCA*. The calculated ρ­(z) profile () agrees qualitatively with the experimental one from SmCA* close to the SmCA* → SmXA* transition (d). It resembles also the experimental profile in SmXA*, despite the layer spacing increases in the hexatic phase, indicating that dimers, present in SmC* and absent in SmCA*, may form again in SmXA*. The ρ­(z) profiles obtained for MIX23HH6 at higher temperatures are closer to a sinusoidal wave than the calculated one, which is explained by low τ l order parameters of the layer order, as was also the case for pure MHPOBC. Summary and Conclusions This study demonstrates that a multicomponent chiral liquid-crystalline system can form a vitrified hexatic smectic phase exhibiting unique dielectric and optical properties. The tertiary mixture MIX23HH6, consisting of MHPOBC, 3F2HPhH6, and 3F3HPhH6 in molar fractions 0.5, 0.25, and 0.25, forms four liquid-crystal smectic phases: A*, C*, CA*, and hexatic XA*, which undergoes a glass transition around 270 K. The SmCA* phase is characterized by a switching time of less than 150 μs down to 348 K and a tilt angle of 35–38° below 368 K. By comparing the temperature dependence of the tilt angle and layer spacing, it is inferred that MHPOBC dimers, which form in the pure compound, are present also in SmC*, but absent in the SmCA* phase of MIX23HH6. Assuming the absence of dimers, an electron density profile perpendicular to the smectic layers is obtained from molecular models optimized by the DFT method, which is in qualitative agreement with the experimental density profile determined from the intensities of diffraction peaks deep in SmCA*. SRL is observed in all tilted smectic phases of MIX23HH6. SmC* shows SRL of mainly blue light. SmCA* shows SRL with a wavelength decreasing on cooling, from 826 nm (red light) at 326 K to 375 nm (blue light) at 308 K; the last point is already in the region of the SmCA*/SmXA* transition. The range of SRL in SmCA* is shifted to higher temperatures by ca. 20–25 K on heating. SmXA* gives a dark blue image under the microscope in the reflection mode, suggesting that SRL occurs in the UV light, just below the visible region. A change to a dark red image occurs shortly before the glass transition of SmXA*, which remains an open question. Another unexpected observation is an apparent absence of the α-process in SmXA*, which is currently explained by overlapping with the β process. Additional measurements for the pure components 3F2HPhH6 and 3F3HPhH6 indicate the formation of SmXA*, although it occurs either during crystallization or in a partially crystallized sample, and the SmXA* glass is not obtained even at the highest cooling rate of 40 K/min. Relaxation processes were observed for both compounds in the crystalline state. The corresponding energy barriers of 30–70 kJ/mol suggest an origin in intramolecular rotations and qualify these crystal phases as CONDIS phases. DSC and XRD results for 3F3HPhH6 suggest that another smectic phase may be present in a very narrow temperature range between SmCA* and the isotropic liquid, but it could not have been identified. Future work will focus on additional 3FmHPhH6/MHPOBC systems, particularly the observation of α- and β-relaxation processes in SmXA*, and the search for mixtures showing SRL in the visible range in SmXA*, which will facilitate the study of helical ordering in this phase. The associated data set is available at 10.48733/IFJPAN/YO1RVG in the RODBUK repository. The Supporting Information is available free of charge at https://pubs.acs.org/doi/10.1021/acs.jpcb.6c02873. - Figures S1–S10: POM textures of MIX23HH6 and 3FmHPhH6 (m = 2, 3) in the transmission mode with numerical analysis; Figures S11, S12: isoconversional analysis of crystallization of 3FmHPhH6 (m = 2, 3); Figures S13–S15: molecular models of 3FmHPhH6 (m = 2, 3) and MHPOBC with corresponding electron density profiles; Figures S16–S19: POM textures of MIX23HH6 in the reflection mode with numerical analysis (PDF) A.D.conceptualization, investigation, formal analysis, funding acquisition, writingoriginal draft. A.D.investigation, writingreview and editing. M.P.investigation, writingreview and editing. M.C.investigation, writingreview and editing. M.F.investigation, writingreview and editing. M.P.investigation, writingreview and editing. E.J.-G.investigation, writingreview and editing The authors declare no competing financial interest.