Colossal Magnetic‐Field‐Induced Anomalous Hall Conductivity in a Kagome Antiferromagnet YMn6Sn6 Minhyuk Choi, Hoil Kim, Minki Sung, Hyeongwoo Seo, Joonyoung Choi, Jaeyoung Kim, Younjung Jo, Han Woong Yeom, Kyung‐Hwan Jin, Jun Sung Kim Abstract Kagome‐lattice magnets provide a fertile ground for exploring exotic electronic phases due to topological band structures and complex magnetic orders. Yet, how these ingredients dictate unconventional magnetotransport responses, crucial for possible spintronic applications, has remained elusive. Here, we show that a prototypical kagome antiferromagnet YMn6Sn6 exhibits significant magnetic‐field‐driven redistribution of Berry curvature and the colossal anomalous Hall conductivity (AHC). Under high magnetic fields, spin canting induces a pronounced spin splitting of the flat and Dirac bands near the Fermi level, dramatically enhancing the Berry curvature. The resulting AHC reaches ∼ 2.5 × 10 S/cm, far exceeding the intrinsic Berry curvature predictions and ranking among the highest reported in magnetic systems. This colossal AHC enhancement is attributed to a synergy between field‐tuned Berry curvature and enhanced skew scattering in the clean limit. Our findings highlight the critical role of magnetic‐field‐controlled spin splitting in engineering Berry curvature and anomalous magnetotransport in clean kagome magnets. Magnetic‐field‐driven spin canting in the kagome antiferromagnet YMn6Sn6 reshapes flat and Dirac bands near the Fermi level, redistributing Berry curvature and producing colossal anomalous Hall conductivity. The study reveals how magnetic configuration and clean‐limit skew scattering cooperate to amplify Hall transport, offering a route to tune topological responses in kagome magnets. [ADVS-9999-e77738-g006.webp] Introduction Kagome‐lattice magnets have recently attracted extensive attention due to their potential to host exotic magnetotransport phenomena [, ]. The kagome lattice, composed of corner‐sharing triangles, inherently supports distinct electronic structures including Dirac cones [, , , , , , ], flat bands [, , , , , ], and van Hove singularities [, , , , ], providing nontrivial topological states and substantial Berry curvature effects. Furthermore, strong geometrical magnetic frustration, intrinsic to kagome lattices, often stabilizes nontrivial magnetic orders, such as noncollinear antiferromagnetism [, , , , , , , , , , , , ], spin liquids [, ], and skyrmion lattices [, ]. Consequently, these topological electronic features, coupled with complex spin textures, can lead to anomalous transport properties such as large anomalous Hall effects (AHE) [, , , , , , ] and topological Hall effects (THE) [, , , ], making kagome magnets promising candidates for next‐generation spintronic devices. However, understanding the underlying mechanism of their rich magnetotransport behaviors has remained elusive. Among recently explored kagome magnets, YMn6Sn6 has emerged as a prototypical kagome antiferromagnet hosting complex magnetic structures, including an incommensurate spiral magnetic order and magnetic‐field‐induced spin canting, which significantly influence its magnetotransport properties [, , , , , , , , ]. Previous studies reported a large AHE with strong variation with external magnetic field, which has been attributed to the THE, explained by magnon‐induced spin scalar chirality at high temperatures []. However, first‐principles calculations have predicted the presence of a Dirac band near the Fermi level in YMn6Sn6, subsequently confirmed via angle‐resolved photoemission spectroscopy (ARPES) []. This Dirac band originating from the kagome lattice implies a possible intrinsic Berry curvature contribution to the observed AHE, but such a possibility has been largely overlooked. Additionally, due to its high electrical conductivity at low temperatures, extrinsic contributions like skew scattering cannot be neglected [, , ]. Consequently, the origin behind the pronounced AHE and its strong magnetic field dependence are unclear, calling for further experimental and theoretical investigations. Here, we combine detailed magnetotransport measurements, ARPES, and density functional theory (DFT) calculations to investigate the magnetic‐field‐induced modulation of momentum (k)‐space Berry curvature and anomalous Hall conductivity (AHC) in YMn6Sn6. We found that strong variation of Berry curvature is induced by systematic changes of the spin‐polarized Dirac bands near the Fermi level due to spin canting. The dramatic enhancement of the AHC of YMn6Sn6 both above and below magnetic saturation fields at low temperatures is attributed to this Berry curvature modulation, amplified by skew scattering in the clean limit. The resulting record high AHC of YMn6Sn6 demonstrates that the interplay of k‐space Berry curvature and the associated skew scattering offers a promising route to enhancing the magnetotransport responses in kagome magnets. Electronic and Magnetic Properties YMn6Sn6 crystallizes into a hexagonal kagome structure with space group P6/mmm, characterized by alternating layered arrangements as depicted in Figure . Mn atoms form distinct kagome planes, sandwiched by Sn‐only and mixed Y‐Sn layers, in an alternating stacking sequence. This structural arrangement is critical for stabilizing various magnetic orders with competing exchange interactions, reflected in the complex field‐dependent magnetic structures (Figure ). Magnetization measurements on our single crystals reveal an antiferromagnetic phase transition at Néel temperature TN ≈ 345 K and also significant anisotropy between the in‐plane (ab‐plane) and out‐of‐plane (c‐axis) directions (Figure ), in good agreement with the previous reports [, , , , , ]. Temperature‐dependent electrical resistivity along the ab‐plane and c‐axis, denoted as ρxx and ρzz, respectively, exhibit clear metallic behaviors (Figure ). The residual resistivity ratio ρ(300 K)/ρ(5 K) reaches to ∼ 44 for ρzz and ∼ 30 for ρxx. These results are also comparable with those reported in the previous experimental reports [, , , , , ]. The resulting conductivity at low temperatures reaches ∼2.1×105 S/cm, and ∼1.5×105 S/cm, for ρzz and ρxx, respectively, which are similar to those of many ferromagnets close to the clean regime []. These observations indicated that in a high quality single crystal of YMn6Sn6, extrinsic scattering contribution, including skew scattering, can be significant for the observed AHE, discussed in detail below. The low temperature phase of YMn6Sn6 exhibits an incommensurate magnetic order with a distorted spiral structure. Under in‐plane magnetic fields, this distorted spiral (DS) changes to the transverse conical spiral (TCS) phases. Upon further increasing the magnetic field, transitions into fan‐like (FL), and intermediate (I) phases, accompanied by distinct spin configurations as illustrated schematically in Figure . Eventually, forced ferromagnetic (FF) phases are observed above the magnetization saturation field. Our magnetization measurements M(H) taken at 5 K for H ∥ ab show four distinct anomalies at H ≈ 2.5, 7.0, 9.9, and 10.5 T, which are more clearly visible in the field‐derivative curve dM(H)/dH and is consistent with the previously established magnetic phase diagram [, , , , , , , ]. For H ∥ c, in contrast, spin canting in the DS phase results in monotonic field dependence of M(H) below the saturation field at ∼ 13.5 T. Excellent agreement with the previous reports confirms the good quality of our crystals [, , , , , ]. Electronic Structure Without Magnetic Fields To capture the essential low‐energy physics of YMn6Sn6 while maintaining computational feasibility, we modeled the experimentally reported incommensurate “distorted spiral” magnetic structure by a commensurate double‐layer antiferromagnetic (AFM) configuration (Figure ). In this model, Mn spins within each kagome bilayer are ferromagnetically aligned, while successive bilayers are coupled antiferromagnetically along the c‐axis, requiring a doubling of the primitive unit cell in the z‐direction. This approximation preserves the key interlayer exchange symmetry breaking while avoiding the computational complexity of fully incommensurate spin textures. The resulting spin‐orbit‐coupled band structure (Figure ) exhibits characteristic kagome‐derived electronic features, including Dirac‐like dispersions, nearly flat bands, and saddle point features. Importantly, these kagome‐derived bands exhibit distinct orbital characters. The Dirac‐like bands closest to the Fermi level near the K point are predominantly derived from Mn dz2 orbital. In contrast, the flat band observed around E≈−0.4 eV is dominated by the in‐plane Mn dxy and dx2−y2 orbitals, while additional flat‐band features farther from the Fermi level contain substantial dyz and dxz contributions. This orbital‐selective character reflects the multi‐orbital nature of the kagome electronic structure in YMn6Sn6. To verify the commensurate double‐layer AFM configuration, we measured ARPES spectra and compared them with the corresponding DFT calculations. Figure shows the ARPES spectra measured along high‐symmetry directions on the kagome‐terminated surface, which exhibit excellent agreement with DFT calculations incorporating the double‐layer AFM ordering, including the overall band dispersion and Dirac‐like dispersions near the K points. We further identify a flat band with a binding energy of 0.3– 0.4 eV (Figure ), another electronic fingerprint of the kagome lattice. The flat band exhibits strong dependence on the polarization of incident light, appearing only in the linear vertical (LV) polarization, which selectively excites in‐plane orbitals (Figure ). Consistently, DFT calculations show that the flat band near −0.4 eV, close to the Fermi level, is dominantly derived from the dxy and dx2−y2 orbitals. These agreements indicate that the commensurate double‐layer AFM model reliably captures essential features of the experimentally observed electronic structures in YMn6Sn6. Additional spectral features in the experiments are attributed to Sn surface states, as identified in the Fermi surface and Sn 4d core‐level spectra (Figure ). Distinct electronic structures can arise depending on the cleavage surface were noticed previously [, , , ]. Electronic Structure Modulation by Field‐Induced Spin Canting Having established the electronic structures at zero magnetic field, we now focus on the effect of an in‐plane magnetic field on the double‐layer AFM ground state. Compared to the response to an out‐of‐plane magnetic field, the more complex evolution of the magnetic structure under an in‐plane field (Figure ) is accompanied by a pronounced nonmonotonic field dependence of the Hall response, as discussed below, thereby providing a more direct basis for comparison between theory and experiment. To model it, we introduce a uniform spin canting angle θ, defined as the rotation of Mn spins from their zero‐field AFM orientation toward the field direction (Figure and Figure S). This approach captures the gradual transformation from AFM (θ=0∘) to FM ordering (θ=90∘) with increasing field strength. Two effects are expected from this spin canting on the electronic structure. First, systematic increase of spin splitting by Zeeman effect as net magnetic moment increases by spin canting. The other is band folding by unit cell doubling along the kz direction in double‐bilayer AFM configuration (Figure ) weakens and eventually disappears in the FF phase with a single bilayer in the unit cell. The calculated Mn dz2‐projected band structures (Figure and Figure ) indeed reveal that the kagome‐derived flat bands undergo progressive spin splitting and approach the Fermi level as θ increases. This shift is accompanied by enhanced dispersion along kz, reflecting the evolution toward interlayer FM alignment. The schematic in Figure summarizes these θ‐dependent band changes, highlighting the downward movement and spin splitting of the flat bands. The systematic variation of the low energy structures with spin canting leads to significant modulation of Berry curvature. As shown in Figure , we calculated the Berry curvature distribution |Ωxz| in the kz=0 plane. For θ=70∘, large Berry curvature hotspots appear near the M point (Figure and Figure ), in stark contrast to the relatively weak distribution at θM=10∘. This enhancement is linked to a pronounced spin‐orbit coupling (SOC)‐induced gap along the M–L direction at the Fermi level for θM≈70∘ (Figure ), as confirmed by the sharp peak in Berry curvature along M‐L (Figure and Figure ). The calculated quantum AHC σzx exhibits a strong θM dependence (Figure ), peaking near θM≈70∘ in line with the Berry curvature maximum. This trend persists even when the Fermi level is shifted by ±50 meV, indicating robustness against moderate carrier doping. These results suggest that field‐induced spin canting in YMn6Sn6 can tune Berry curvature in the momentum space through controlled modification of the kagome band topology. Thus the field‐induced magnetic phase transitions, associated with jumps in the M(H) (Figure ) and spin canting angle θM result in the significant changes in the k‐space Berry curvature. Colossal Anomalous Hall Conductivity To address the strong field‐dependent Berry curvature effect, we investigated the magnetotransport properties under different magnetic field orientations. Insets in Figures illustrate schematic diagrams of two measurement configurations used for the magnetotransport experiments: one for the longitudinal (ρxx) and transverse (ρyx) resistivities with magnetic fields (H∥z∥[001]) and current (I∥x∥[100]) applied along the z‐ and x‐axes, respectively, and the other for the longitudinal (ρzz) and transverse (ρxz) resistivities with H∥y and I∥z. Clear anisotropic and nonmonotonic magnetotransport responses are observed under magnetic fields. For H∥z, while the M(H) data shows a smooth increase with magnetic field, clear changes in the slope of the magnetic‐field‐dependent resistivities (ρxx(H) and ρyx(H)) are observed. This observation is consistent with significant variations in the electronic structure at the Fermi level due to spin canting. For H∥y, even more complex magnetic field dependencies of ρzz and ρxz are observed, showing step‐like features associated with field‐induced magnetic phase transitions. These results strongly suggest that magnetotransport properties are sensitive to both electronic structure variations caused by spin canting and the underlying magnetic structures. The Berry curvature effect on magnetotransport can be monitored by AHC as shown in Figure . To quantify the AHC, we first separate the ordinary Hall component, which arises from the Lorentz force‐driven charge deflection, from the measured transverse resistivities (ρyx and ρxz). For both configurations, the Hall resistivity can be described by ρH=ρN+ρA=RHB+ρA [, , , , , , , ], where RH is the Hall coefficient and ρA is the anomalous contribution. The value of RH was obtained by fitting the data in the high‐field regions, H>13.5 T for H∥z and H>10.7 T for H∥y, where the magnetization is saturated, allowing ρA to be treated as a field‐independent constant. These fittings yield RH ∼ 4.9 × 10 cm3/C for H∥z and RH ∼ 2.6 × 10 cm3/C for H∥y, typical values of metals with large Fermi surfaces. We note that while the limited field range above Hsat for H∥z may introduce minor uncertainty in RH, the obtained RH value for H∥y is reliable due to a sufficiently wide fitting range. Subsequently, the AHC, σijA, is calculated by subtracting the normal contribution σijN=RHB/ρ2 from the total Hall conductivity σij, using the relationship σijA≈−ρijA/(ρiiρjj), where i and j represent respective crystallographic axes. The resulting anomalous component σxzA, illustrated as the black line in Figure , exhibits significant variation with magnetic field, reaching a maximum value of ∼2.5×104 S/cm in the FL phase. These values are much larger than typical AHC values found in various magnetic materials [, , ]. The pronounced enhancement, distinct anisotropy, and field‐dependent evolution of the AHC clearly highlight the critical roles of field‐induced spin canting, Berry curvature redistribution, and nontrivial magnetization structures in governing the magnetotransport properties of YMn6Sn6. Let us focus on the AHC for H∥y, σxzA, in YMn6Sn6 at magnetic fields above the magnetization saturation field in the FF phase. As shown in Figure , σxzA reaches ∼5.0×103 S/cm, larger than the highest AHC values reported to date for ferromagnets e.g., ∼1.6×103 S/cm in Ni [], ∼2.0×103 S/cm in Co2MnGa [], ∼2.5×103 S/cm in Fe‐doped CoS2 [], and ∼2.9×103 S/cm in NdCrSb3 []. This colossal AHC value far exceeds the intrinsic Berry‐curvature limit e2/ha≈1.0×103 S/cm [, ] and is nearly ∼ 23 times larger than the calculated intrinsic AHC for the FF phase of YMn6Sn6. In this FF phase, THE contribution from spin scalar chirality is negligible, because it vanishes with fully aligned spin moments. Instead, this unusually large enhancement can be due to extrinsic mechanisms, most likely impurity skew scattering in the clean limit [, ]. With a longitudinal conductivity approaching ∼106S/cm, YMn6Sn6 indeed lies in a regime where such extrinsic contributions can dominantly contribute to the AHC. Nevertheless, we found that the enhancement factor ∼23 of the measured AHC with respect to the Berry curvature calculation is an order of magnitude larger than in the colossal AHE materials mentioned above, with the typical enhancement ratio of ∼1−4 [, , , ]. Hence, conventional skew scattering driven solely by spin–orbit coupling at impurity sites cannot account for the observed colossal AHC in YMn6Sn6. Berry Curvature‐Induced Skew Scattering A more plausible explanation invokes skew‐scattering contributions that are strongly enhanced by Berry curvature, even in the absence of SOC at impurity sites. As shown in Ref. [], finite Berry curvature induces a noncommutative nature of electron wavefunctions in the real space, producing asymmetric scattering probabilities and thus a significant increase in the AHC. In this framework, the asymmetric scattering rate obeys Wasym∝niV3ΩkF, where ni is the impurity density, V the scalar impurity potential, and ΩkF the Berry curvature at the Fermi wavevector. By contrast, in conventional skew scattering driven by SOC at the impurity site, Wasym∝niV2λimp, with λimp the SOC strength at the impurity sites. Consequently, the ratio of the two resulting anomalous Hall conductivities satisfies σyxBC,skσyximp,sk∝VΩkFλimp, where σyxBC,sk and σyximp,sk correspond to the AHC contributions from Berry‐curvature‐enhanced skew scattering and impurity skew scattering, respectively. Taking typical values V∼0.1–1 eV, ΩkF∼102–103/Å2, and λimp∼0.05–1 eV /Å, this ratio can reach 101–102, indicating that Berry‐curvature‐induced skew scattering is far more effective at amplifying the AHC than conventional impurity‐driven skew scattering. A recent study on colossal AHC of Fe‐ and Ni‐doped CoS2 indeed reveals significantly enhanced AHC than the Berry curvature prediction in the clean limit. The doping dependence of this skew‐scattering‐enhanced AHC shows an intimate correlation with the calculated Berry curvature [], supporting the dominant role of Berry‐curvature‐induced skew scattering. We therefore attribute the remarkably large AHC observed in the FF phase of YMn6Sn6 to the combined effect of intrinsic Berry curvature and Berry‐curvature‐enhanced skew scattering in the clean regime. Below the magnetization saturation field in the FL phases, we observe an even stronger enhancement of σxzA, reaching up to ∼2.5×104 S/cm at H=9.5 T. In the previous studies, the THE has been attributed to scalar spin chirality generated by magnetic fluctuations [] or nontrivial spin textures []. However, the pronounced enhancement of σxzA observed in the FL phase, rather than in the TCS phase, at low temperatures cannot be primarily ascribed to the THE. First, magnetic fluctuations capable of generating scalar spin chirality are expected to be nearly quenched at low temperatures and high magnetic fields, as theoretically confirmed in a recent study []. Second, scalar spin chirality should be sizable in the TCS phase owing to its conical spiral spin configuration, whereas it should be strongly suppressed in the FL phase, where the spin configuration has a negligible solid angle in spin space. Consistent with this expectation, recent high‐field neutron diffraction experiments reported scalar spin chiralities of −0.726 at 2 K and 5 T and −0.864 at 240 K and 3 T in the TCS phase []. Although these sizable values would suggest a finite THE contribution in the TCS phase, no clear THE signature is observed at low temperatures, in contrast to the pronounced enhancement of σxzA found in the FL phase in our experiments. Therefore, while a minor THE contribution to the AHC cannot be completely ruled out, it is unlikely to be the dominant origin of the colossal σxzA below the saturation field. The monotonous increase of σyxA(H) with magnetic field also supports minor contribution of the THE below the saturation field. Under magnetic field applied along the c‐axis, the Mn moments continuously cant from the ab‐plane toward the c direction as shown in Figure , without an additional field‐induced magnetic transition. If the THE contribution due to the finite scalar spin chirality is dominant, σyxA(H) would become largest at an intermediate noncoplanar spin configuration and then diminish as the moments approach the collinear FF phase. Experimentally, however, σyxA(H) increases monotonically with magnetic field and remains largest in the FF phase, where the fully aligned moments produce no scalar spin chirality (Figure ). This behavior further supports the conclusion that the measured Hall responses are dominated by the AHE rather than by the THE contribution. The observed colossal AHC below the saturation field can instead be attributed to the pronounced dependence of the Berry curvature on the spin‐canting angle. As shown in Figure , the calculated Berry‐curvature contribution to σxzA exhibits a maximum near H∼9.5 T, consistent with the field at which the experimental σxzA reaches its peak. This field‐tunable Berry curvature can strongly enhance σxzA through the skew‐scattering channel, as discussed above for the FF phase. By assuming the same enhancement factor of ∼23 obtained for the FF phase, the renormalized σxzA reproduces the experimentally observed peak structure in Figure . Although this analysis relies on an approximate double‐AFM spin configuration and a field‐independent enhancement factor, the qualitative agreement between the experimental and calculated σxzA highlights the important role of spin‐canting‐angle‐dependent Berry curvature. These observations suggest that the complex field dependence and the colossal enhancement originate from the synergistic effects of strongly field‐tunable k‐space Berry curvature and Berry‐curvature‐driven skew scattering as the system approaches the clean limit. The resulting AHC in YMn6Sn6 reaches ∼2.5×104 S/cm, among the highest values reported for magnetic materials. Figure compares the absolute AHC, |σAHE|, with the longitudinal conductivity, σxx, for YMn6Sn6 and representative ferromagnetic, kagome, and frustrated magnetic systems [, , , , , , , , , , , , , , , , ]. For both Hall components of YMn6Sn6, σxzA for H∥y and σyxA for H∥z, the AHC lies well above the conventional intrinsic Berry‐curvature scale of ∼103 S/cm, while the corresponding longitudinal conductivities place YMn6Sn6 close to the clean transport regime, where skew scattering is expected to scale approximately linearly with σxx. Moreover, the maximum |σAHE| values of YMn6Sn6 exceed most reported values for frustrated magnets, with the notable exception of the recent record value reported for the ultraclean frustrated antiferromagnet PdCrO2 []. These observations indicate that the observed AHC cannot be accounted for by the intrinsic Berry‐curvature contribution or by a real‐space topological Hall contribution alone, and instead point to a substantial extrinsic amplification of AHC near the clean regime. We note that the colossal AHC in PdCrO2 has been attributed to spin‐cluster skew scattering by fluctuating clusters of localized spins with finite scalar spin chirality, a contribution that is strongly amplified in the clean limit []. Together with our findings in YMn6Sn6, this comparison suggests that clean‐limit skew scattering, despite its distinct microscopic origins, provides a general route to enhancing the AHC. In conclusion, we demonstrate that, in kagome antiferromagnets, field‐induced changes in spin configuration, including spin canting, can substantially modify the low‐energy electronic band structure and generate strongly field‐dependent Berry curvature in momentum space. This finding challenges the commonly adopted assumption that the AHC arising from momentum‐space Berry curvature should scale proportionally with the field‐dependent magnetization [, , , , , , , ]. Within this conventional framework, any additional contribution deviating from the σA(H)∝M(H) behavior is often attributed to a THE driven by field‐induced scalar spin chirality in real space. However, kagome antiferromagnets host flat bands and Dirac band crossings near the Fermi level, which act as strong sources of k‐space Berry curvature. Even subtle modifications of these electronic structures caused by spin canting can therefore produce a complex field dependence of the AHC. This effect is further enhanced as the system approaches the clean limit, where Berry‐curvature‐induced skew scattering can amplify the contribution from k‐space Berry curvature. The colossal AHC and its strong magnetic‐field tunability in YMn6Sn6 thus reveal a complex interplay between magnetic configuration and momentum‐space Berry curvature in kagome antiferromagnets. Methods Single Crystal Growth and Physical Property Measurements Single crystals of YMn6Sn6 were grown using a Sn‐flux method with a Canfield crucible. The stoichiometric mixture (1:6:30) of Y chips (99.99%), Mn powder (99.99%), and Sn shot (99.99%) was loaded in a sealed quartz tube under vacuum and loaded into a box furnace at 1000 for 24 h, cooled down to 600 and centrifuged. Flat and shiny crystals were obtained, of which crystallinity and stoichiometry were confirmed by X‐ray diffraction and energy‐dispersive X‐ray spectroscopy (Figure ). Magnetization was measured under a magnetic field along the c‐axis or ab‐plane using a vibrating sample magnetometer of Physical Property Measurement System (PPMS‐14T, Quantum Design). The conventional six‐probe method was employed for the resistivity measurements. The samples were measured in a Physical Property Measurement System (Quantum Design). We attached gold wires on a rectangular‐shaped sample and applied the current (I) along a‐axis or c‐axis and measured voltages (Vmea) in longitudinal and transverse directions while sweeping magnetic fields (H) from 14 T to ‐14 T. The longitudinal (Rxx,zz(H)) and transverse (Ryx,xz(H)) resistances are extracted from the data taken with positive and negative magnetic fields, using Rxx,zz(H)=[Vmea(H)+Vmea(−H)]/2I and Ryx,xz(H)=[Vmea(H)−Vmea(−H)]/2I. Angle‐Resolved Photoemission Spectroscopy ARPES measurements were conducted at the 4A2 beamline of the Pohang Light Source using a DA30L electron analyzer (Scienta Omicron, Sweden) and at the 4.0.3 beamline of Advanced Light Source. Crystal was cleaved under ultrahigh vacuum (base pressure < 1 × 10−10 Torr) to obtain clean surfaces. At the Pohang Light Source, both cleaving and measurements were performed at 70 K, whereas at the Advanced Light Source, cleaving and measurements were carried out at 10 K. Furthermore, measurements with a photon energy of 138 eV and both linear‐horizontal (LH) and linear‐vertical (LV) polarizations were performed on the kagome termination to analyze orbital characters in detail. Density Functional Theory Calculations We performed first‐principles calculations within the framework of DFT using the Perdew–Burke–Ernzerhof‐type generalized gradient approximation for the exchange‐correlation functional, as implemented in the Vienna ab initio simulation package [, ]. All calculations were carried out using the kinetic energy cutoff of 520 eV on a 12 × 12 × 4 Monkhorst–Pack k‐point mesh for the double‐layer AFM spin configuration of YMn6Sn6. The intrinsic anomalous Hall conductivity is calculated based on the Wannier90 code [, ] with d orbitals of Mn atoms and p orbital of Sn atoms. The k mesh for intrinsic Hall conductivity calculation is 130 × 130 × 30 with adaptive refinement mesh of 5 × 5 × 5.