Compression-shear behavior of high-resistance backfill walls in gob-side entry retaining for thick seams Authors: Lei Sun, Fan Qiao, ShuaiShuai Jiang, Chong Li Published: 2026 ABSTRACT To address the insufficient bearing capacity of roadside backfill bodies and the tilting or failure induced by uneven pressure relief of the coal seam during gob-side entry retaining in thick coal seams with hard roofs, combined compression–shear loading tests incorporating rapid resistance build-up and varying inclination angles were performed. A novel Compression Shear Coupling Test system (CSCT) was developed, and a fitted relationship between backfill width and roof subsidence was established. The strength degradation behavior of backfill specimens subjected to different shear stress components was systematically investigated. The results reveal that the peak strength of the specimens declines with increasing shear stress component, and the failure mode transitions progressively from compressive to shear-dominated failure. The high-resistance backfill material derived from this study was implemented at the N2302 gob-side entry retaining working face, accompanied by an anti-tilting design for the backfill wall. The measured roof subsidence was reduced by 59.4% relative to the theoretically predicted value, and no evident signs of failure or deterioration were observed in the backfill body. These findings provide both data support and theoretical reference for gob-side entry retaining under similar mining conditions. Introduction Gob-side entry retaining, as a pillar-less mining technique, can significantly improve the coal resource recovery rate, alleviate the imbalance between excavation and extraction, and enhance underground ventilation conditions. It has therefore received extensive attention and application in thick coal seam mining both domestically and internationally1–4. However, for gob-side entry retaining under a hard roof in a thick coal seam, the roof typically exhibits large thickness, high strength, wide hanging area, and large breaking interval, resulting in significant lateral abutment pressure on the goaf side and intense dynamic pressure effects5–9. As the key load-bearing structure of gob-side entry retaining, the roadside backfill body directly withstands the rotation, subsidence, and shearing action of the roof strata, and its mechanical performance and stability are the core factors determining the success or failure of the retained entry10–14. Field practices indicate that under a hard roof in a thick coal seam, conventional backfill bodies commonly suffer from three prominent issues. First, the insufficient early-age load-bearing capacity of the backfill body makes it difficult to rapidly increase resistance so as to restrain the severe early roof subsidence. Second, the large mining height in thick coal seam extraction induces significant horizontal displacement and overturning moment among the roof, backfill body, and floor; together with the uneven compressive deformation of the coal seam itself, this easily causes overturning instability of the backfill body. Third, during the rotation of the key block formed after hard roof breakage, a non-negligible shear stress component is imposed on the backfill body. This shear stress, acting in combination with the vertical compressive stress, accelerates shear failure of the backfill body and seriously threatens the safety of the retained entry15–19. Therefore, revealing the damage evolution laws of the backfill body under combined compression-shear stress states, and developing backfill materials with both high early strength and good deformation adaptability, have become critical scientific issues to be urgently addressed. To tackle these problems, numerous studies have been conducted by domestic and international scholars. Regarding optimization of backfill material proportioning, previous research has investigated the effects of water-to-cement ratio, early-strength agent dosage, and fiber content on the uniaxial or triaxial compressive performance of backfill materials, finding that appropriate addition of early-strength agents and fibers can effectively enhance the early strength and post-peak ductility of the backfill wall20–24. In terms of the mechanical response of backfill bodies, some researchers have analyzed their strength characteristics, deformation behavior, and failure modes through uniaxial, conventional triaxial, and cyclic loading–unloading tests25–28. However, most of these studies are based on pure compression or quasi-static loading conditions, failing to fully account for the realistic combined compression-shear stress path induced during the rotation and subsidence of a hard roof. In practice, the sidewall of the backfill body for gob-side entry retaining is commonly subjected to both the inclined shear force from the roof and the vertical compressive stress, and its stress state is closer to combined compression-shear loading29–31. To date, systematic experimental studies on the strength degradation law of backfill bodies under different shear stress components remain very limited, and dedicated testing equipment capable of applying controlled shear stress is lacking. Moreover, existing anti-overturning designs mostly focus on increasing the strength of the backfill body itself or widening the wall, whereas research on the overall stability control method of the backfill body under combined compression-shear loading is still incomplete. In view of this, this study takes the N2302 working face of the Gucheng Coal Mine, which features a thick coal seam and a hard roof, as the engineering background. Systematic combined compression-shear loading tests are carried out on the roadside backfill wall material for gob-side entry retaining. First, a novel Compression Shear Coupling Test system (CSCT) loading system is developed to achieve stable loading under different preset shear stress components. Second, the backfill material proportion is optimized through orthogonal tests, obtaining material parameters that enable rapid resistance increase and high early strength. Then, combined compression-shear loading tests at different inclination angles (i.e., different shear stress components) are performed to reveal the degradation laws of shear stress on the peak strength, peak strain, and failure mode of the backfill body. Finally, the optimized high-resistance backfill body is applied in the field, with corresponding anti-overturning technical measures designed to verify its engineering applicability. The research findings aim to provide a theoretical basis and experimental data support for the design and stability control of backfill bodies for gob-side entry retaining under hard roofs in thick coal seams, as well as for engineering applications under similar conditions. Project overview At the N2302 working face, top-coal caving is conducted along the floor of the No. 3 coal seam. The working face exhibits a general topographic dip from south to north, with the No. 3 coal seam approximating a monoclinal structure. The average dip angle is 5°, and the burial depth ranges from 530 to 600 m. The total thickness of the coal seam varies between 3.35 and 9.37 m, averaging 6.35 m. The immediate roof of the coal seam is mainly composed of sandy mudstone and mudstone, with local siltstone intercalations. Its thickness ranges from 0 to 7.45 m (average 4.03 m), characterized by poor thickness stability, a loose structure, water-softening behavior, and low strength. The immediate floor consists of sandy mudstone, mudstone, and locally siltstone, classified as soft rock, with a thickness varying from 0 to 2.45 m (average 0.70 m). The N2302 working face has a length of 302 m. The belt entry of the working face is designed as a gob-side entry retaining, with a roadway width of 6 m and a height of 3.8 m. A 1.5-m-wide C30 concrete wall is adopted as the retaining structure for the gob-side entry. The layout of the working face is presented in Fig. 1.Fig. 1Layout of the working face. Layout of the working face. Materials and methods Backfill material parameters Concrete material parameters The experiments were based on the mix proportion of the C30 concrete used for the roadside packing body at the N2302 working face of Gucheng Coal Mine (Table 1). The baseline mass ratio of coarse aggregate (gravel), sand, and cementitious material was 9:8:5.5. Specimens were prepared with varying water‑cement ratios, fiber contents, and dosages of an early‑strength agent. The cement used was P.O42.5 ordinary Portland cement. The sand was medium sand (Zone II), water‑washed, and sieved through a 0.45 mm mesh, with a mud or stone powder content of less than 3%. The gravel was 5–10 mm continuously graded pebble, with a mud content of less than 1% and a stone powder content of less than 0.5%. The raw materials are shown in Fig. 2.Table 1Preliminary mix proportion for pumped concrete.Concrete gradeBinderGravelSandWaterC30550 kg900 kg800 kg220 kgFig. 2Raw materials used in the test. Table 1Preliminary mix proportion for pumped concrete.Concrete gradeBinderGravelSandWaterC30550 kg900 kg800 kg220 kg Preliminary mix proportion for pumped concrete. Raw materials used in the test. Water‑cement ratio parameters The water‑cement (w/c) ratio directly affects concrete strength. A high w/c ratio dilutes the colloidal hydration products of the cementitious material, preventing adequate filling of voids between concrete particles. Conversely, a low w/c ratio leads to incomplete hydration and agglomeration of the cementitious material, resulting in internal voids. Moreover, the concrete paste becomes overly thick, exhibits poor fluidity, and is difficult to mix, all of which significantly reduce concrete strength. To determine the optimal w/c ratio under the test conditions, six gradient levels (0.35, 0.40, 0.45, 0.50, 0.55, and 0.60) were tested in preliminary trials. These tests established a suitable w/c range to inform the w/c parameters for subsequent orthogonal experiments. The test mixes consisted of cement, sand, and water, stirred until homogeneous. The experimental parameters are listed in Table 2.Table 2Preliminary experimental parameters for water-cement ratio.Water–cement ratioSand (g)Cement (g)Water (g)0.35820.0561.4196.00.40812.5562.5237.50.45800.0550.0247.00.50792.1544.6272.30.55783.5538.7296.30.60775.2533.0319.8 Table 2Preliminary experimental parameters for water-cement ratio.Water–cement ratioSand (g)Cement (g)Water (g)0.35820.0561.4196.00.40812.5562.5237.50.45800.0550.0247.00.50792.1544.6272.30.55783.5538.7296.30.60775.2533.0319.8 Preliminary experimental parameters for water-cement ratio. Figure 3 shows the morphology of pastes with different w/c ratios. According to the test results shown in Fig. 3, at a w/c ratio of 0.35, the material exhibited distinct granular particles, accompanied by large unmixed lumps, a very dry surface, and no cohesion. At w/c = 0.40, the material changed from large lumps to small lumps, still with obvious granular particles, a dry surface, and no cohesion. At w/c = 0.45, the granular particles disappeared, the surface was relatively dry, initial cohesion appeared, but fluidity was poor. At w/c = 0.50, the material surface was moist, cohesion was evident, and a certain fluidity was observed. At w/c = 0.55, a small amount of liquid exuded on the surface, cohesion was clear, the material appeared semi‑pasty, and flowability was good. At w/c = 0.60, the material was distinctly pasty, with obvious liquid exudation on the surface, strong fluidity, and good cohesion. Based on the above results, the first three w/c ratios (0.35–0.45) gave poor performance and lacked fluidity, failing to meet the requirements for flexible‑formwork concrete backfilling. The last three ratios (0.50–0.60) exhibited good cohesion and flowability, making them suitable for orthogonal testing and flexible‑formwork concrete backfilling. Therefore, three w/c gradients were selected for the main experiments: 0.50, 0.55, and 0.60.Fig. 3Morphology of slurries with different water‑cement ratios. Morphology of slurries with different water‑cement ratios. Fiber Basalt fiber (Fig. 4) was selected as the target fiber material. Basalt fiber is manufactured by drawing natural basalt rock at high temperatures. It offers advantages such as high production capacity, abundant raw materials, low cost, and environmental friendliness. In addition, basalt fiber exhibits excellent mechanical properties, including good wear resistance, oxidation resistance, compressive strength, and shear strength. Because the fiber is made from basalt, it has high rock affinity and can effectively enhance the crack resistance and fatigue resistance of concrete.Fig. 4Chopped Basalt Fiber. Chopped Basalt Fiber. Fiber content was set at three levels: 0%, 0.3%, and 0.6% by volume of the concrete block. The fiber density ranges from 2.65 to 3.0 g/cm3; a value of 2.8 g/cm3 was used to calculate the fiber mass for each content level. Long fibers tend to bend and agglomerate during mixing, reducing their toughening effect on concrete. Therefore, 6‑mm chopped fibers were used throughout the tests. These experiments investigated the effect of fiber content on concrete strength. Early‑strength agent content Industrial‑grade calcium formate (Fig. 5) was selected as the concrete early‑strength agent. Three dosages (0%, 0.6%, and 1.2% by mass of the cementitious material) were tested to evaluate the improvement in early‑age (7‑day) strength of concrete.Fig. 5Calcium Formate Concrete Early-Strength Agent Diagram. Calcium Formate Concrete Early-Strength Agent Diagram. CSCT test apparatus The CSCT system used in this study was developed based on the C-CAST system at the University of New South Wales32–34. A new pin connection structure was designed and incorporated into the adapters of the CSCT system to match the loading end of the MTS testing machine at China University of Mining and Technology, thereby eliminating the loosening and slippage issues associated with rope fixation in the original system. In addition, the cylindrical variable‑angle fixture was redesigned into a cubic version suitable for cubic specimens. The cubic specimen is fixed by pre‑set limiting grooves within the fixture. Both the upper and lower adapters consist of a base and a matching positioning dial; the two adapters are identical in structure and are arranged symmetrically during testing. The physical and three‑dimensional structural diagrams of the new CSCT system are shown in Fig. 6.Fig. 6Diagram of the novel CSCT system structure (1: Pin structure; 2: Adapter; 3: Positioning scale; 4: Fixing screw components; 5: Sample; 6: Limiting slot) (a) Schematic diagram of the three-dimensional structure (b) Photograph of the actual system. Diagram of the novel CSCT system structure (1: Pin structure; 2: Adapter; 3: Positioning scale; 4: Fixing screw components; 5: Sample; 6: Limiting slot) (a) Schematic diagram of the three-dimensional structure (b) Photograph of the actual system. The installation of the test system involves the following four steps:Rotate the upper and lower positioning dials to the required test angles and secure them to the corresponding adapters using bolts.Place the cured cubic specimen into the limiting groove of the lower adapter. The groove has a designed depth of 10 mm to prevent specimen slippage due to dimensional tolerances, thereby ensuring test precision.Connect the upper adapter to the loading end of the MTS testing machine via its pin connection structure, enabling servo‑controlled loading of the specimen.Slightly adjust the MTS testing machine to slowly lower the limiting groove of the upper adapter onto the top of the specimen, thus fixing both the top and bottom ends of the specimen within the grooves to prevent any sliding. Rotate the upper and lower positioning dials to the required test angles and secure them to the corresponding adapters using bolts. Rotate the upper and lower positioning dials to the required test angles and secure them to the corresponding adapters using bolts. Place the cured cubic specimen into the limiting groove of the lower adapter. The groove has a designed depth of 10 mm to prevent specimen slippage due to dimensional tolerances, thereby ensuring test precision. Place the cured cubic specimen into the limiting groove of the lower adapter. The groove has a designed depth of 10 mm to prevent specimen slippage due to dimensional tolerances, thereby ensuring test precision. Connect the upper adapter to the loading end of the MTS testing machine via its pin connection structure, enabling servo‑controlled loading of the specimen. Connect the upper adapter to the loading end of the MTS testing machine via its pin connection structure, enabling servo‑controlled loading of the specimen. Slightly adjust the MTS testing machine to slowly lower the limiting groove of the upper adapter onto the top of the specimen, thus fixing both the top and bottom ends of the specimen within the grooves to prevent any sliding. Slightly adjust the MTS testing machine to slowly lower the limiting groove of the upper adapter onto the top of the specimen, thus fixing both the top and bottom ends of the specimen within the grooves to prevent any sliding. Once the installation is complete, the loading scheme can be set for subsequent tests. Given that the undulating slope of the gob‑side entry retaining wall at Gucheng Coal Mine and the inclination angle of the backfill body are generally small, three test gradients (10°, 15°, and 20°) were selected for compression‑shear strength testing in this study. Strength calculation principle As illustrated in Fig. 7, during a combined compression–shear loading test, an angular deviation exists between the loading direction and the axial orientation of the specimen. Under this configuration, the axial stress, axial strain, and shear stress acting on the specimen are defined as follows:1\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\sigma_{\alpha } = \frac{F}{S}\cos \alpha$$\end{document}2\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\varepsilon_{\alpha } = \frac{{H_{1} - H_{2} }}{H}$$\end{document}3\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\tau_{\alpha } = \frac{F}{S}\sin \alpha$$\end{document}where σα represents the axial stress of the backfill specimen, εα denotes the axial strain; τα is the resolved shear stress component; F corresponds to the vertical load applied by the testing apparatus; S is the initial cross-sectional area of the specimen; H1 refers to the original specimen height; and H2 denotes the height following compression.Fig. 7Force diagram of the inclined loading test. Force diagram of the inclined loading test. Influence of backfill width on roadway deformation To evaluate the effect of backfill width on roadway convergence behavior and to substantiate the support efficacy of the high-resistance backfill material, a mechanical model was developed based on the principle of energy conservation. This model characterizes the relationship between the rotational subsidence of the rigid roof strata and the reactive support provided by the backfill body. Accordingly, a functional correlation between roof displacement (Δl) and backfill width (b) was established. In accordance with the principle of energy conservation, the total work performed by the rotational movement of the main roof and immediate roof is equivalent to the sum of the work done by the internal roadway support resistance, the work contributed by the roadside backfill support force, and the strain energy accumulated within both the immediate roof and the coal wall. This equilibrium is expressed as:4\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$W_{z1} = W_{b} + W_{z2} + W_{n} + W_{c}$$\end{document} In this expression, Wz1 denotes the total work performed by the overlying strata load on the immediate roof during rotational subsidence, in addition to the work performed by the self-weight of the immediate roof; Wb​ denotes the strain energy stored within the coal wall resulting from compressive deformation induced by roof rotation; Wz2 denotes the strain energy stored within the immediate roof; Wn​ denotes the work done by the roadway support resistance acting on the immediate roof; and Wc denotes the work done by the roadside backfill support resistance acting on the immediate roof. The detailed derivation of Eq. (4) is presented in Appendix A. By combining Equations (A1) through (A6), the following expression is obtained:5\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\begin{gathered} \frac{1}{2}\left( {q_{1} \tan \theta \left( {x_{0} + a + b} \right)^{2} + m_{z} g\left( {x_{0} + a + b} \right)\sin \theta } \right) = \frac{{K_{b} x_{0}^{3} \Delta l^{2} }}{{6(x_{0} + {\raise0.7ex\hbox{$a$} \!\mathord{\left/ {\vphantom {a 2}}\right.\kern-0pt} \!\lower0.7ex\hbox{$2$}})^{2} }} \hfill \\ \quad + \frac{{h_{z} x_{0}^{3} \Delta l^{2} K_{b}^{2} }}{{4E_{z} (x_{0} + {\raise0.7ex\hbox{$a$} \!\mathord{\left/ {\vphantom {a 2}}\right.\kern-0pt} \!\lower0.7ex\hbox{$2$}})^{2} }} + f_{s} a\Delta l + f_{d} b\frac{{x_{0} + a + {\raise0.7ex\hbox{$b$} \!\mathord{\left/ {\vphantom {b 2}}\right.\kern-0pt} \!\lower0.7ex\hbox{$2$}}}}{{x_{0} + {\raise0.7ex\hbox{$a$} \!\mathord{\left/ {\vphantom {a 2}}\right.\kern-0pt} \!\lower0.7ex\hbox{$2$}}}}\Delta l \hfill \\ \end{gathered}$$\end{document} The above result can be rearranged into a quadratic equation with respect to Δl, which takes the standard form:6\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$A\Delta l^{2} + B\Delta l + C = 0$$\end{document}where the coefficients are defined as:7\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\left\{ {\begin{array}{*{20}l} {A = \frac{{K_{b} x_{0}^{3} }}{{6(x_{0} + {\raise0.7ex\hbox{$a$} \!\mathord{\left/ {\vphantom {a 2}}\right.\kern-0pt} \!\lower0.7ex\hbox{$2$}})^{2} }} + \frac{{h_{z} x_{0}^{3} K_{b}^{2} }}{{4E_{z} (x_{0} + {\raise0.7ex\hbox{$a$} \!\mathord{\left/ {\vphantom {a 2}}\right.\kern-0pt} \!\lower0.7ex\hbox{$2$}})^{2} }}} \\ {B = f_{s} a + f_{d} b\frac{{x_{0} + a + {\raise0.7ex\hbox{$b$} \!\mathord{\left/ {\vphantom {b 2}}\right.\kern-0pt} \!\lower0.7ex\hbox{$2$}}}}{{x_{0} + {\raise0.7ex\hbox{$a$} \!\mathord{\left/ {\vphantom {a 2}}\right.\kern-0pt} \!\lower0.7ex\hbox{$2$}}}}} \\ {C = - \frac{1}{2}\left( {q_{1} \tan \theta \left( {x_{0} + a + b} \right)^{2} + m_{z} g\left( {x_{0} + a + b} \right)\sin \theta } \right)} \\ \end{array} } \right.$$\end{document} Substituting the relevant parameters into Eq. (7) and solving the quadratic equation for Δl yields the functional relationship between the roof displacement (Δl) and the backfill width (b). The fitted functional relationship between roadway roof displacement and backfill width is expressed as:8\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\Delta l = 44.64 + \frac{2557.59}{{1 + \left( {{\raise0.7ex\hbox{$b$} \!\mathord{\left/ {\vphantom {b {0.53}}}\right.\kern-0pt} \!\lower0.7ex\hbox{${0.53}$}}} \right)^{1.23} }}$$\end{document} The fitted curve illustrating the relationship between roof deformation (Δl) and varying backfill widths (b) is presented in Fig. 8. As observed from the curve, the roof displacement decreases with increasing backfill width; however, the rate of decrease progressively diminishes. Specifically, the roof displacement reaches approximately 1000 mm at a backfill width of 0.8 m, and remains at approximately 450 mm even at the maximum backfill width of 2.0 m. This indicates that, in gob-side entry retaining within thick coal seams, increasing the backfill width can reduce the deformation of the surrounding rock to a certain extent. Nevertheless, a wider backfill does not equate to proportionally better performance, as the influence of increased width on surrounding rock deformation gradually attenuates. While the specific values may vary under different geological conditions, the general trend remains consistent.Fig. 8Influence curve of backfill width on roadway roof displacement. Influence curve of backfill width on roadway roof displacement. Experimental scheme Based on the key parameters identified above, an L9 (34) orthogonal array was adopted for the experiments. The test scheme is presented in Table 3. Group Y specimens involved three factors: fiber content, water‑cement (w/c) ratio, and early‑strength agent content. Group J specimens involved four factors: fiber content, inclination angle, w/c ratio, and early‑strength agent content.Table 3L₉ (34) Orthogonal experimental design with four factors and three levels.GroupFiber content (%)Blank control / Inclination angle (°)Water-cement ratioEarly‑strength agent dosage (%)Y1/J10100.500Y2/J20150.550.6Y3/J30200.601.2Y4/J40.3100.551.2Y5/J50.3150.600Y6/J60.3200.500.6Y7/J70.6100.600.6Y8/J80.6150.501.2Y9/J90.6200.550 Table 3L₉ (34) Orthogonal experimental design with four factors and three levels.GroupFiber content (%)Blank control / Inclination angle (°)Water-cement ratioEarly‑strength agent dosage (%)Y1/J10100.500Y2/J20150.550.6Y3/J30200.601.2Y4/J40.3100.551.2Y5/J50.3150.600Y6/J60.3200.500.6Y7/J70.6100.600.6Y8/J80.6150.501.2Y9/J90.6200.550 L₉ (34) Orthogonal experimental design with four factors and three levels. Concrete specimens were prepared using C30 concrete with three w/c ratios (0.50, 0.55, 0.60), three basalt fiber contents (0%, 0.3%, 0.6%), and three calcium formate (early‑strength agent) dosages (0%, 0.6%, 1.2% by mass of cementitious material), following an L9 (34) orthogonal combination. Uniaxial compression tests were conducted at 7 d and 28 d, and compression‑shear tests were performed at three inclination angles (10°, 15°, and 20°). Nine groups (Y1–Y9) were designated for uniaxial compression, and another nine groups (J1–J9) for variable‑angle compression‑shear tests. To minimize experimental error, each group was tested in duplicate. All specimens measured 100 mm × 100 mm × 100 mm. Specimen preparation and testing procedure Specimen preparation followed the Chinese standard for concrete specimen making and curing (GB/T50081‑2019). Specimens were prepared in two batches for 7‑d and 28‑d testing, respectively; the preparation process is shown in Fig. 9. During preparation, materials were weighed and mixed according to the experimental parameters. The molds were oiled to facilitate demolding. After concrete placement, the molds were vibrated on a vibrating table to compact the concrete. Vibration continued until the surface showed paste, and no large bubbles emerged, thereby reducing the influence of internal voids on test accuracy. After molding, the specimen surfaces were troweled to ensure flatness. The specimens were demolded 24 h later and immediately placed into a standard curing chamber at 20 °C ± 2 °C and a relative humidity > 95%. Finally, 7‑d and 28‑d concrete specimens were obtained.Fig. 9Diagram of Concrete Specimen Preparation Process. Diagram of Concrete Specimen Preparation Process. Figure 10 shows the test loading system. Both uniaxial compression tests and combined compression‑shear loading tests were conducted. All tests employed a loading rate of 0.5 mm/min and a data sampling frequency of 30.0 Hz. For uniaxial compression, the specimen was placed at the center of the compression platen. The loading system was adjusted via the control system and an adjustment module to bring it into near contact with the specimen, after which loading commenced until specimen failure. For variable‑angle compression‑shear tests, the protractor on the variable‑angle device was adjusted to set the compression‑shear angle to 10°, 15°, or 20°. The specimen was placed at the center of the device, with its lower‑right and upper‑left corners engaging the specimen holder in the dip direction, followed by test loading.Fig. 10Test loading system. Test loading system. Results and discussion Analysis of uniaxial compressive strength and resistance-increasing characteristics Macroscopic failure characteristics under uniaxial compression Figure 11 illustrates the failure modes of the concrete specimens under uniaxial compression, while Fig. 12 presents the corresponding mechanical response curves. As observed, the unreinforced specimens exhibited severe crack propagation, extensive macroscopic spalling, and a high degree of fragmentation. In contrast, the specimens reinforced with 0.3% and 0.6% basalt fibers demonstrated restricted crack development, maintained robust overall structural integrity, and showed no significant block detachment.Fig. 11Uniaxial compression failure morphology of specimens.Fig. 12Uniaxial compressive stress–strain curves of specimens. Uniaxial compression failure morphology of specimens. Uniaxial compressive stress–strain curves of specimens. Mechanistically, unreinforced specimens are susceptible to rapid crack coalescence and localized spalling after reaching peak strength, which is characteristic of a pronounced brittle failure mode. The incorporation of basalt fibers introduces a three-dimensional, randomly distributed bridging network within the cementitious matrix. During the initiation and propagation of microcracks, these fibers mitigate further crack extension via bridging, pull-out, and frictional energy dissipation, thereby retarding the formation of macroscopic fracture planes. Furthermore, the interfacial bonding between the fibers and the matrix continues to transfer tensile and shear stresses during the post-peak stage. This mechanism enables the specimen to preserve substantial integrity and residual load-bearing capacity even beyond peak strength. Correlating these observations with the 28-day mechanical response curves reveals that the load-bearing capacity of the unreinforced specimens (Y1, Y2, and Y3) declined precipitously post-peak, indicating inferior residual strength. Conversely, specimens with 0.3% and 0.6% fiber contents exhibited a more gradual post-peak stress drop and superior structural cohesion. Therefore, the fundamental contribution of basalt fibers lies not merely in enhancing crack initiation resistance, but more critically in augmenting post-peak toughness and fracture resistance. This enhancement is of paramount importance for maintaining the structural stability and load-bearing capacity of backfill walls in gob-side entry retaining subjected to continuous roof subsidence. Peak strain Peak strain reflects the deformation resistance of a material. Figure 13 presents the peak strain values for different mix proportions. With increasing curing time, the peak strain of the 28‑d groups increased to a certain extent compared to the 7‑d groups. Among all groups, Y6 (w/c = 0.50, early‑strength agent = 0.6%, fiber = 0.3%) exhibited relatively larger peak strain. In the 7‑d groups, Y4 (w/c = 0.55, early‑strength agent = 1.2%, fiber = 0.3%) had the smallest peak strain, while in the 28‑d groups, Y5 (w/c = 0.60, early‑strength agent = 0%, fiber = 0.3%) showed the smallest peak strain. These results indicate that peak strain is jointly influenced by w/c ratio, early‑strength agent content, and fiber content. Among the tested groups, the mixed proportion of Y6 provided the greatest improvement in peak strain.Fig. 13Peak strain of different groups. Peak strain of different groups. Peak strength Table 4 lists the uniaxial compressive strength of concrete at 7 d and 28 d, and Fig. 14 shows the strengths and their ratios. The average 7‑d uniaxial compressive strength ranged from 19.28 to 26.84 MPa, and the average 28‑d strength from 30.08 to 34.26 MPa. The 7‑d strength reached 63–78% of the 28‑d strength. Among specimens with identical fiber content, w/c ratio, and early‑strength agent dosage, the 7‑d/28‑d strength ratio was 73% for Y2 (no fiber), 78% for Y6 (0.3% fiber), and 71% for Y7 (0.6% fiber)—the highest values within their respective fiber content groups. All three groups had an early‑strength agent level of 2 (i.e., 0.6% dosage). In contrast, groups without an early‑strength agent and those with 1.2% dosage showed less pronounced strength improvement: Y5 and Y4, as well as Y9 and Y8, had comparable strengths, while Y3 exhibited a significant strength reduction compared to Y1. This indicates that an appropriate amount of early‑strength agent can notably enhance early‑age strength, whereas excessive dosage is not beneficial and may even reduce it.Table 4Uniaxial compressive strength at 7 and 28 days.Specimen NoFailure load/(kN)28‑d uniaxial compressive strength/(MPa)Average/(MPa)Specimen NoFailure load/(kN)7‑d uniaxial compressive strength /(MPa)Average/(MPa)Y1345.1033.9732.12Y1-7251.4822.5322.33306.7830.26254.5422.12Y2328.0432.6632.80Y2-7251.9124.8324.04335.1932.93235.5023.24Y3312.4130.9530.72Y3-7191.4819.0619.28311.9230.49196.6419.50Y4339.2332.9633.52Y4-7229.8522.7122.88349.0834.07235.5823.05Y5306.0030.0130.08Y5-7212.3320.9620.46306.4530.14203.1919.96Y6357.9235.2834.26Y6-7272.7227.2126.84336.5433.24267.3426.46Y7316.1331.4031.46Y7-7220.3922.3322.40319.9431.52208.9922.47Y8367.5535.6333.87Y8-7249.4823.9323.29330.1332.11237.1222.64Y9332.5132.1032.25Y9-7234.3022.4622.16331.8532.40232.7921.86Fig. 14Uniaxial Compressive Strength at 7 and 28 Days and Their Ratio. Table 4Uniaxial compressive strength at 7 and 28 days.Specimen NoFailure load/(kN)28‑d uniaxial compressive strength/(MPa)Average/(MPa)Specimen NoFailure load/(kN)7‑d uniaxial compressive strength /(MPa)Average/(MPa)Y1345.1033.9732.12Y1-7251.4822.5322.33306.7830.26254.5422.12Y2328.0432.6632.80Y2-7251.9124.8324.04335.1932.93235.5023.24Y3312.4130.9530.72Y3-7191.4819.0619.28311.9230.49196.6419.50Y4339.2332.9633.52Y4-7229.8522.7122.88349.0834.07235.5823.05Y5306.0030.0130.08Y5-7212.3320.9620.46306.4530.14203.1919.96Y6357.9235.2834.26Y6-7272.7227.2126.84336.5433.24267.3426.46Y7316.1331.4031.46Y7-7220.3922.3322.40319.9431.52208.9922.47Y8367.5535.6333.87Y8-7249.4823.9323.29330.1332.11237.1222.64Y9332.5132.1032.25Y9-7234.3022.4622.16331.8532.40232.7921.86 Uniaxial compressive strength at 7 and 28 days. Uniaxial Compressive Strength at 7 and 28 Days and Their Ratio. Range and variance analysis Tables 5, 6, 7, 8 present the range and variance analyses for the 7‑d and 28‑d uniaxial compressive strength. The range analysis of 7‑d strength ranks the influencing factors as: w/c ratio > early‑strength agent content > fiber content. The optimal parameters are w/c ratio level 1, early‑strength agent level 2, and fiber content level 2, i.e., w/c = 0.50, early‑strength agent = 0.6%, and fiber = 0.3%. The variance analysis for 7‑d strength shows P‑values of 0.022 (fiber), 0.004 (w/c), and 0.005 (early‑strength agent), all less than α = 0.05. Thus, the null hypothesis—that different levels of each factor have no significant effect on the test index—is rejected, indicating that all three factors significantly affect the 7‑d strength. Similarly, the range and variance analysis for the 28‑d strength yields the same ranking: w/c ratio > early‑strength agent content > fiber content, with the same optimal mix (w/c = 0.50, early‑strength agent = 0.6%, fiber = 0.3%). The variance analysis results are also significant. Notably, the early‑strength agent significantly affects the 28-day strength, suggesting that it not only improves early‑age strength but also optimizes the internal composition of concrete, thereby exerting a significant influence on the final strength.Table 5Range analysis of uniaxial compressive strength at 7 days.NoFiber content groupControl groupWater‑cement ratio groupEarly‑strength agent content group\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${K}_{1}$$\end{document}65.6467.6172.4464.95\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${K}_{2}$$\end{document}70.1767.7869.0873.27\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${K}_{3}$$\end{document}67.8468.2762.1465.44k121.8822.5424.1521.65k223.3922.5923.0324.42k322.6122.7620.7121.81R1.510.223.432.77Table 6Analysis of variance for uniaxial compressive strength at 7 days.Source of varianceSum of squaresDegrees of freedomMean squareF-valueP-valueSignificanceFiber content3.4221.7144.060.022P < 0.05 (Significant)Control group0.0820.041.000.500–Water‑cement ratio18.4129.20236.970.004P < 0.05 (Significant)Early‑strength agent dosage14.5327.26187.020.005P < 0.05 (Significant)Table 7Range analysis of uniaxial compressive strength at 28 days.NoFiber content groupControl groupWater‑cement ratio groupEarly‑strength agent content groupK195.6397.09100.2594.44K297.8596.7398.5698.51K397.5897.2392.2598.11k131.8832.3633.4231.48k232.6232.2432.8532.84k332.5332.4130.7532.70R0.740.172.671.36Table 8Analysis of variance for uniaxial compressive strength at 28 days.Source of varianceSum of squaresDegrees of freedomMean squareF-valueP-valueSignificanceFiber content0.9820.4922.270.043P < 0.05(Significant)Control group0.0420.021.000.500–Water‑cement ratio11.8425.92269.330.004P < 0.05 (Significant)Early‑strength agent dosage3.3521.6776.200.013P < 0.05 (Significant) Table 5Range analysis of uniaxial compressive strength at 7 days.NoFiber content groupControl groupWater‑cement ratio groupEarly‑strength agent content group\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${K}_{1}$$\end{document}65.6467.6172.4464.95\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${K}_{2}$$\end{document}70.1767.7869.0873.27\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${K}_{3}$$\end{document}67.8468.2762.1465.44k121.8822.5424.1521.65k223.3922.5923.0324.42k322.6122.7620.7121.81R1.510.223.432.77 Range analysis of uniaxial compressive strength at 7 days. Table 6Analysis of variance for uniaxial compressive strength at 7 days.Source of varianceSum of squaresDegrees of freedomMean squareF-valueP-valueSignificanceFiber content3.4221.7144.060.022P < 0.05 (Significant)Control group0.0820.041.000.500–Water‑cement ratio18.4129.20236.970.004P < 0.05 (Significant)Early‑strength agent dosage14.5327.26187.020.005P < 0.05 (Significant) Analysis of variance for uniaxial compressive strength at 7 days. Table 7Range analysis of uniaxial compressive strength at 28 days.NoFiber content groupControl groupWater‑cement ratio groupEarly‑strength agent content groupK195.6397.09100.2594.44K297.8596.7398.5698.51K397.5897.2392.2598.11k131.8832.3633.4231.48k232.6232.2432.8532.84k332.5332.4130.7532.70R0.740.172.671.36 Range analysis of uniaxial compressive strength at 28 days. Table 8Analysis of variance for uniaxial compressive strength at 28 days.Source of varianceSum of squaresDegrees of freedomMean squareF-valueP-valueSignificanceFiber content0.9820.4922.270.043P < 0.05(Significant)Control group0.0420.021.000.500–Water‑cement ratio11.8425.92269.330.004P < 0.05 (Significant)Early‑strength agent dosage3.3521.6776.200.013P < 0.05 (Significant) Analysis of variance for uniaxial compressive strength at 28 days. According to the analysis, Y6 is the optimal mix. Compared to Y1, Y6 exhibits a 2.14 MPa increase in 28‑d uniaxial compressive strength and a 4.50 MPa increase in 7‑d strength. The ratio of 7‑d to 28‑d strength increases from 70 to 78%, indicating better early‑age resistance increase and significant strength improvement. Analysis of strength damage behavior under variable‑angle compression‑shear conditions Macroscopic failure characteristics As shown in Fig. 15, which illustrates the failure modes on the front and back faces, the first group without fiber exhibited a higher degree of fragmentation than the other groups, confirming that fiber addition enhances crack resistance. Specimens subjected to 10° compression‑shear generally showed a high degree of failure, with numerous longitudinal through‑cracks but fewer lateral through‑cracks. As the compression‑shear angle increased to 15° and 20°, the degree of fragmentation gradually decreased, longitudinal through‑cracks diminished, and lateral through‑cracks increased. After failure at 20°, the specimens maintained good overall integrity, exhibiting only a pronounced trend of single‑crack lateral through‑failure. Since the shear failure strength of concrete is much lower than its compressive failure strength, this indicates that during compression‑shear loading from 10° to 20°, the failure mode gradually transitions from compression‑dominated to shear‑dominated.Fig. 15Failure morphology of specimens under compression‑shear coupled loading. Failure morphology of specimens under compression‑shear coupled loading. Peak strength Table 9 presents the compression‑shear strengths at 7 d and 28 d. Figure 16 shows the 7‑d and 28‑d compression‑shear strengths, and their ratios, and Fig. 17 shows the ratios of compression‑shear strength to uniaxial compressive strength.Table 9Shear-compression strength at 7 and 28 days.Specimen NoFailure load/(kN)28‑d compression‑shear strength/(MPa)Average/(MPa)Specimen NoFailure load/(kN)7‑d compression‑shear strength /(MPa)Average/(MPa)J1235.6723.2423.01J1-7184.9518.1417.87231.2722.77181.1017.60J2218.6821.5520.97J2-7173.3517.0017.50210.3320.40181.8918.00J3173.6117.2316.85J3-7117.3611.6511.51166.8316.47115.0311.38J4224.1522.0122.28J4-7171.0516.7116.44229.0222.56163.4016.17J5196.1219.7919.72J5-7140.5113.8014.24198.5519.65147.6514.67J6213.5121.2021.18J6-7193.8318.4217.38215.7421.15166.7216.33J7218.1321.7219.77J7-7149.0814.6015.18219.1021.81156.9715.75J8234.2622.8722.66J8-7152.7415.5715.44229.8822.45150.3515.30J9186.3318.7818.6J9-7134.2513.0312.65189.0518.42129.3812.27Fig. 16Compression‑shear strength of specimens at 7 d and 28 d under combined loading and their ratios.Fig. 17Ratio of compression‑shear strength to uniaxial compressive strength at 7 d and 28 d. Table 9Shear-compression strength at 7 and 28 days.Specimen NoFailure load/(kN)28‑d compression‑shear strength/(MPa)Average/(MPa)Specimen NoFailure load/(kN)7‑d compression‑shear strength /(MPa)Average/(MPa)J1235.6723.2423.01J1-7184.9518.1417.87231.2722.77181.1017.60J2218.6821.5520.97J2-7173.3517.0017.50210.3320.40181.8918.00J3173.6117.2316.85J3-7117.3611.6511.51166.8316.47115.0311.38J4224.1522.0122.28J4-7171.0516.7116.44229.0222.56163.4016.17J5196.1219.7919.72J5-7140.5113.8014.24198.5519.65147.6514.67J6213.5121.2021.18J6-7193.8318.4217.38215.7421.15166.7216.33J7218.1321.7219.77J7-7149.0814.6015.18219.1021.81156.9715.75J8234.2622.8722.66J8-7152.7415.5715.44229.8822.45150.3515.30J9186.3318.7818.6J9-7134.2513.0312.65189.0518.42129.3812.27 Shear-compression strength at 7 and 28 days. Compression‑shear strength of specimens at 7 d and 28 d under combined loading and their ratios. Ratio of compression‑shear strength to uniaxial compressive strength at 7 d and 28 d. The 7‑d compression‑shear strength at different angles ranges from 11.51 to 17.87 MPa, and the 28‑d strength ranges from 16.85 to 23.01 MPa. Compared to uniaxial compressive strength, the compression‑shear strength is significantly lower. The 7‑d compression‑shear strength is only 57–80% of the uniaxial compressive strength, and the 28‑d strength is only 55%–72%. As shown in Fig. 15, with increasing compression‑shear angle, both the 7‑d and 28‑d ratios decrease markedly, and the rate of decrease accelerates. Notably, for the first three groups, the 7‑d ratio drops from 80 to 60%, and the 28‑d ratio drops from 72 to 55%, indicating a substantial strength reduction. This suggests that when the backfill body has a certain inclination or is placed in an inclined environment, it is subjected to combined compressive and shear stresses from the roof and floor, resulting in significant strength degradation. Under such conditions, the backfill body is more prone to failure, and this tendency becomes more pronounced with increasing inclination angle. Additionally, concrete specimens with early‑strength agent level 2 (0.6% dosage) exhibited relatively higher 7‑d compression‑shear strength, reaching up to 83% of the 28‑d strength, indicating that an appropriate amount of early‑strength agent can notably enhance the early‑age strength of the concrete backfill body. Range and variance analysis Tables 10, 11, 12 and 13 present the range and variance analyses for the 7‑d and 28‑d compression‑shear strength. For 7‑d compression‑shear strength, the factors are ranked as: w/c ratio > compression‑shear angle > early‑strength agent content > fiber content. The optimal parameters are w/c = 0.50, compression‑shear angle = 10°, early‑strength agent = 0.6%, and fiber = 0.3%. The P‑values from the variance analysis for all factors are less than α, indicating that variations in each factor significantly affect the 7‑d strength.Table 10Range analysis of shear-compression strength at 7 days.NoFiber content groupCombined compression‑shear loading groupWater–cement ratio groupEarly‑strength agent content groupK193.7798.97101.3689.51K296.1094.3493.18100.10K386.5283.0881.8586.78\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${k}_{1}$$\end{document}15.6316.5016.8914.92\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${k}_{2}$$\end{document}16.0215.7215.5316.68\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${k}_{3}$$\end{document}14.4213.8513.6414.46R1.602.653.252.22Table 11Analysis of variance for shear-compression strength at 7 Days.Source of varianceSum of squaresDegrees of freedomMean squareF-valueP-valueSignificanceFiber content8.322.004.168.558.29e−3P < 0.05 (Significant)Inclination angle22.262.0011.1322.892.95e−4P < 0.05 (Significant)Water‑cement ratio32.002.0016.0032.897.27e−5P < 0.05 (Significant)Early‑strength agent dosage16.502.008.2516.968.84e−4P < 0.05 (Significant)sse24.389.000.490.041.00–Table 12Range analysis of shear-compression strength at 28 days.NoFiber content groupCombined compression‑shear loading groupWater–cement ratio groupEarly‑strength agent content groupK1121.66134.11133.68122.65K2126.36126.71123.72127.83K3126.05113.25116.67123.59k120.2822.3522.2820.44k221.0621.1220.6221.31k321.0118.8819.4520.60R0.783.482.840.86Table 13Analysis of variance for shear-compression strength at 28 Days.Source of varianceSum of squaresDegrees of freedomMean squareF-valueP-valueSignificanceFiber content2.302.001.157.511.21e−2P < 0.05 (Significant)Inclination angle37.282.0018.64121.583.07e−7P < 0.05 (Significant)Water‑cement ratio24.352.0012.1779.401.92e−6P < 0.05 (Significant)Early‑strength agent dosage2.542.001.278.289.13e−3P < 0.05 (Significant)sse21.389.000.150.011.00– Table 10Range analysis of shear-compression strength at 7 days.NoFiber content groupCombined compression‑shear loading groupWater–cement ratio groupEarly‑strength agent content groupK193.7798.97101.3689.51K296.1094.3493.18100.10K386.5283.0881.8586.78\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${k}_{1}$$\end{document}15.6316.5016.8914.92\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${k}_{2}$$\end{document}16.0215.7215.5316.68\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${k}_{3}$$\end{document}14.4213.8513.6414.46R1.602.653.252.22 Range analysis of shear-compression strength at 7 days. Table 11Analysis of variance for shear-compression strength at 7 Days.Source of varianceSum of squaresDegrees of freedomMean squareF-valueP-valueSignificanceFiber content8.322.004.168.558.29e−3P < 0.05 (Significant)Inclination angle22.262.0011.1322.892.95e−4P < 0.05 (Significant)Water‑cement ratio32.002.0016.0032.897.27e−5P < 0.05 (Significant)Early‑strength agent dosage16.502.008.2516.968.84e−4P < 0.05 (Significant)sse24.389.000.490.041.00– Analysis of variance for shear-compression strength at 7 Days. Table 12Range analysis of shear-compression strength at 28 days.NoFiber content groupCombined compression‑shear loading groupWater–cement ratio groupEarly‑strength agent content groupK1121.66134.11133.68122.65K2126.36126.71123.72127.83K3126.05113.25116.67123.59k120.2822.3522.2820.44k221.0621.1220.6221.31k321.0118.8819.4520.60R0.783.482.840.86 Range analysis of shear-compression strength at 28 days. Table 13Analysis of variance for shear-compression strength at 28 Days.Source of varianceSum of squaresDegrees of freedomMean squareF-valueP-valueSignificanceFiber content2.302.001.157.511.21e−2P < 0.05 (Significant)Inclination angle37.282.0018.64121.583.07e−7P < 0.05 (Significant)Water‑cement ratio24.352.0012.1779.401.92e−6P < 0.05 (Significant)Early‑strength agent dosage2.542.001.278.289.13e−3P < 0.05 (Significant)sse21.389.000.150.011.00– Analysis of variance for shear-compression strength at 28 Days. For 28‑d compression‑shear strength, the factors are ranked as: compression‑shear angle > w/c ratio > early‑strength agent content > fiber content. This indicates that the inclination angle has the greatest influence on the strength of the backfill body. Optimizing the material mix can enhance its compression‑shear performance. The optimal parameters are compression‑shear angle = 10°, w/c = 0.50, early‑strength agent = 0.6%, and fiber = 0.3%. The P‑values from the variance analysis for all factors are also less than α, demonstrating that variations in each factor significantly improve the 28‑d strength. These results confirm that appropriate w/c ratio, early‑strength agent dosage, and fiber content can markedly enhance the compression‑shear strength of the backfill body. Industrial test Field test Crack initiation and strength deterioration in the backfill body typically occur at an early stage before it attains a certain load‑bearing capacity. Based on the comparative results between the optimal concrete mix (Y6) and the control group (Y1), a mix proportion with a water‑cement ratio of 0.50, 0.6% early‑strength agent, and 0.3% fiber content was adopted to construct the gob‑side entry retaining wall in the main haulage gateway of the N2302 working face at Gucheng Coal Mine. The wall width was reduced from 1.5 to 1.2 m to lower backfilling costs. In addition, a foundation reinforcement treatment was applied to the bottom area of the backfill body: a groove was excavated in advance, and concrete was poured to form a foundation, thereby enhancing the tilt resistance of the backfill wall. As shown in Fig. 18a, the foundation increases the contact area with the floor coal, reduces the bearing pressure at the bottom, and mitigates tilting induced by floor coal deformation.Fig. 18Construction diagrams of the flexible‑formwork concrete backfill. Construction diagrams of the flexible‑formwork concrete backfill. Meanwhile, temporary support consisting of a one-beam and three-prop structure was combined with the installation of tied anchor bolts within the flexible formwork. Steel strips, bearing plates, and bolts were fastened at both ends of the tied anchors, with an anchor spacing of 800 mm × 900 mm, as illustrated in Fig. 18b. This configuration facilitates the development and exertion of the supporting resistance of the backfill body. Based on the backfill material test results, field backfilling tests were conducted. The construction process of the flexible‑formwork concrete in the N2302 transportation gateway and the on‑site operations are shown in Fig. 18c. Effectiveness verification of the backfill wall Surface displacement monitoring stations were installed using the cross‑point method to measure roadway surface displacements during the entry‑retaining stage, as shown in Figs. 19 and 20. Floor heave was approximately 290 mm, while roof sag and coal rib bulging were about 340 mm and 180 mm, respectively. The overall deformation of the roadway was well controlled. Field photographs also indicate that the backfill body maintained a good supporting shape without signs of bulging failure. The coal rib exhibited no obvious bulging, the overall roadway profile remained intact, and the support components functioned properly without evident failure or damage. These results satisfy the requirements for normal mining operations.Fig. 19Surrounding rock control of the gob‑side entry retaining construction section.Fig. 20Surrounding rock displacement variation in the backfill section of the gob‑side entry retaining. Surrounding rock control of the gob‑side entry retaining construction section. Surrounding rock displacement variation in the backfill section of the gob‑side entry retaining. Conclusions To determine the parameters of a backfill material for gob‑side entry retaining that exhibits rapid resistance increase and high early strength, and to reveal the deterioration patterns of the shear stress component on the peak strength, peak strain, and failure mode of the backfill body, an orthogonal experiment was conducted to develop a high‑strength backfill material for thick coal seams with hard roofs. The following conclusions are drawn:Under uniaxial compression, fiber incorporation significantly improves the integrity and crack resistance of concrete specimens and mitigates post‑peak strength degradation. The 7‑d strength reaches 63%–78% of the 28‑d strength. The group with 0.6% early‑strength agent shows a notable improvement in 7-day strength, whereas excessive early‑strength agent hinders normal strength development.Range and variance analyses of the 7‑d and 28‑d uniaxial compressive strength indicate that the factors are ranked in descending order of influence as: water‑cement ratio > early‑strength agent content > fiber content. The optimal mix proportion is a water‑cement ratio of 0.50, 0.6% early‑strength agent, and 0.3% fiber content. Compared to the original group with the same water‑cement ratio (0.50), the optimal group shows increases of 2.14 MPa and 4.50 MPa in 28‑d and 7‑d compressive strength, respectively, and the 7‑d/28‑d strength ratio increases from 70 to 78%, indicating a significant improvement in early strength.The degree of specimen fragmentation correlates with the evolution of the shear stress component and decreases with increasing inclination angle. As the angle increases from 10° to 20°, longitudinal through‑cracks decrease while lateral through‑cracks increase, and the specimens maintain high integrity with a single‑crack lateral through‑failure characteristic. With a larger angle, the compressive strength reduction becomes more pronounced, and the failure mode progressively transitions from compression‑dominated to shear‑dominated. Appropriate water‑cement ratio, early‑strength agent dosage, and fiber content can effectively enhance the compression‑shear strength of concrete.Following the field application of the optimized high-resistance backfill material and the implementation of corresponding anti-tilting technical measures, the deformation of the roadway surrounding rock was monitored using the cross-point layout method. The monitoring results reveal that the floor heave of the roadway is approximately 290 mm, while the roof subsidence and rib convergence are approximately 340 mm and 180 mm, respectively. With the backfill width reduced to 1.2 m, the measured roof subsidence exhibits a 59.4% reduction relative to the theoretically predicted value. The overall deformation control of the roadway is deemed effective, the backfill support remains structurally stable, and no visible indications of failure or deterioration are observed. Under uniaxial compression, fiber incorporation significantly improves the integrity and crack resistance of concrete specimens and mitigates post‑peak strength degradation. The 7‑d strength reaches 63%–78% of the 28‑d strength. The group with 0.6% early‑strength agent shows a notable improvement in 7-day strength, whereas excessive early‑strength agent hinders normal strength development. Under uniaxial compression, fiber incorporation significantly improves the integrity and crack resistance of concrete specimens and mitigates post‑peak strength degradation. The 7‑d strength reaches 63%–78% of the 28‑d strength. The group with 0.6% early‑strength agent shows a notable improvement in 7-day strength, whereas excessive early‑strength agent hinders normal strength development. Range and variance analyses of the 7‑d and 28‑d uniaxial compressive strength indicate that the factors are ranked in descending order of influence as: water‑cement ratio > early‑strength agent content > fiber content. The optimal mix proportion is a water‑cement ratio of 0.50, 0.6% early‑strength agent, and 0.3% fiber content. Compared to the original group with the same water‑cement ratio (0.50), the optimal group shows increases of 2.14 MPa and 4.50 MPa in 28‑d and 7‑d compressive strength, respectively, and the 7‑d/28‑d strength ratio increases from 70 to 78%, indicating a significant improvement in early strength. Range and variance analyses of the 7‑d and 28‑d uniaxial compressive strength indicate that the factors are ranked in descending order of influence as: water‑cement ratio > early‑strength agent content > fiber content. The optimal mix proportion is a water‑cement ratio of 0.50, 0.6% early‑strength agent, and 0.3% fiber content. Compared to the original group with the same water‑cement ratio (0.50), the optimal group shows increases of 2.14 MPa and 4.50 MPa in 28‑d and 7‑d compressive strength, respectively, and the 7‑d/28‑d strength ratio increases from 70 to 78%, indicating a significant improvement in early strength. The degree of specimen fragmentation correlates with the evolution of the shear stress component and decreases with increasing inclination angle. As the angle increases from 10° to 20°, longitudinal through‑cracks decrease while lateral through‑cracks increase, and the specimens maintain high integrity with a single‑crack lateral through‑failure characteristic. With a larger angle, the compressive strength reduction becomes more pronounced, and the failure mode progressively transitions from compression‑dominated to shear‑dominated. Appropriate water‑cement ratio, early‑strength agent dosage, and fiber content can effectively enhance the compression‑shear strength of concrete. The degree of specimen fragmentation correlates with the evolution of the shear stress component and decreases with increasing inclination angle. As the angle increases from 10° to 20°, longitudinal through‑cracks decrease while lateral through‑cracks increase, and the specimens maintain high integrity with a single‑crack lateral through‑failure characteristic. With a larger angle, the compressive strength reduction becomes more pronounced, and the failure mode progressively transitions from compression‑dominated to shear‑dominated. Appropriate water‑cement ratio, early‑strength agent dosage, and fiber content can effectively enhance the compression‑shear strength of concrete. Following the field application of the optimized high-resistance backfill material and the implementation of corresponding anti-tilting technical measures, the deformation of the roadway surrounding rock was monitored using the cross-point layout method. The monitoring results reveal that the floor heave of the roadway is approximately 290 mm, while the roof subsidence and rib convergence are approximately 340 mm and 180 mm, respectively. With the backfill width reduced to 1.2 m, the measured roof subsidence exhibits a 59.4% reduction relative to the theoretically predicted value. The overall deformation control of the roadway is deemed effective, the backfill support remains structurally stable, and no visible indications of failure or deterioration are observed. Following the field application of the optimized high-resistance backfill material and the implementation of corresponding anti-tilting technical measures, the deformation of the roadway surrounding rock was monitored using the cross-point layout method. The monitoring results reveal that the floor heave of the roadway is approximately 290 mm, while the roof subsidence and rib convergence are approximately 340 mm and 180 mm, respectively. With the backfill width reduced to 1.2 m, the measured roof subsidence exhibits a 59.4% reduction relative to the theoretically predicted value. The overall deformation control of the roadway is deemed effective, the backfill support remains structurally stable, and no visible indications of failure or deterioration are observed.