Controlled polymerization of methyl acrylate in the presence of copper MOF (Basolite®C300): strategy and characterization Authors: Edina Rusen, Cristina Stavarache, Aurel Diacon, Bogdan Vasile, Alexandra Mocanu, Oana Brincoveanu, Gabriela Toader, Cosmin Romanitan, Adina Boldeiu Published: 2026 ABSTRACT The controlled polymerization of methyl acrylate (MA) in the presence of Basolite copper C300 (MOF@Cu) is presented in the present study. MOF@Cu plays a single role, acting as a cocatalyst that is reduced by the copper wire or light (red LED) to produce Cu(I) ions necessary to activate the controlled polymerization. Thus, the polymerization in the presence of Cu(0) wire and MOF@Cu can follow two reaction pathways: SARA-ATRP or SET-LRP. Based on the kinetics investigation, the SET-LRP route is supported by GPC, UV-Vis, and 1H NMR analyses. The percentage of the living chain (26%) was determined using 1H NMR. Under red LED irradiation, photoinduced polymerization leads to the formation of copper nanoparticles, as characterized by BFTEM. Also, using the same initiation procedure, an emulsion was obtained directly via polymerization, and the particles were investigated by SEM.Supplementary InformationThe online version contains supplementary material available at 10.1038/s41598-026-57663-3. Introduction Reversible-deactivation radical polymerization (RDRP) is one of the most modern polymerization techniques1,2. Using this method, polymers with complex architecture can be obtained3–5. From this class of polymerization, it is important to remember atom transfer polymerization (ATRP)6,7, nitroxide-mediated polymerization (NMP)8,9, and reversible addition-fragmentation chain transfer (RAFT)10,11. It can also consider the derivative methods of previously presented types of polymerizations, such as Activator Regenerated by Electron Transfer (ARGET)12–14, Supplemental Activation Reducing Agent (SARA)15,16, Single-Electron Transfer Living Radical Polymerization (SET-LRP)17–19, etc. Reducing agents such as ascorbic acid (AsA), tin(II) 2-ethylhexanoate (Sn(EH)2), hydrazine, glucose, sodium sulphite, iodide ions, phenol derivatives, etc., are used to obtain copper (I) from the copper (II) ions20,21. It is well known that copper(I) acts as an activator in ATRP polymerization. The requirement for such polymerization is that the reducing agent consistently interacts with Cu(II) ions and Pn-X (in SARA ATRP). More recently, our group published studies22–24 regarding the polymerization of methyl methacrylate (MMA) in the presence of halogenated organic derivatives/polymers and copper wire. The mechanism can follow two distinct pathways: one is SARA-ATRP, as highlighted by Matyjaszewski[25,26,27, and the other is SET-LRP, sustained by Percec28,29. The percentage of both mechanisms has been determined. Metal-organic frameworks (MOFs) are hybrid materials that combine inorganic and organic components, characterized by their porous, crystalline, and network-like structures30,31. These frameworks are constructed by coordinating metal ions or clusters with organic ligands. The specific coordination geometries of the metals and ligands influence their diverse periodic arrangements and porosity levels32. A variety of metals and ligands can be employed to design MOFs with tailored properties, making them suitable for applications such as industrial use (gas separation, storage, and adsorption), biomedical (drug delivery, bioimaging, phototherapy), and environmental applications (catalysis)33–35. Using MOFs in RDRP is valuable because of their particle size of a few hundred nanometres; the MOF catalyst can be easily collected by centrifugation and reused for other polymerizations. Additionally, copper-based MOFs can play a dual role, serving as both catalysts and ligands. As previously presented, the mechanism in the presence of a copper wire could be SARA-ATRP or SET-LRP. The main differences between the suggested mechanisms consist of the following36: ❖ in the case of SARA-ATRP, Cu (I) is the main activator, and Cu (0) is a supplemental and reducing agent, in contrast to SET-LRP, where Cu (0) is the activator of the alkyl halide; ❖ comproportionation is specific for SARA-ATRP, and disproportionation for SET-LRP; ❖ in the case of SARA-ATRP, there is limited termination, versus SET-LRP, where zero termination and end group functionality are 100%; ❖ activation step via Inner Sphere Electron Transfer (ISET) for SARA-ATRP, and Outer Sphere Electron Transfer (OSET) for SET-LRP; Both mechanisms are characterized by primary deactivation by Cu(II) and negligible deactivation by Cu(I), as shown in Scheme 1. Scheme 1Comproportionation and disproportionation specific for SARA-ATRP and SET-LRP. Comproportionation and disproportionation specific for SARA-ATRP and SET-LRP. Also, as a reducing agent for Cu (II), it could be an external stimulus, like light37. It is well known in the specific literature concerning the photo-induced ATRP reactions38–40. Thus, the second objective of our study was to highlight the importance of the red LED (λ = 630 nm) (1 mW/cm2) on the polymerization of methyl acrylate (MA) in the presence of MOF@Cu. The polymerization in the presence of light is purer than in the presence of Cu(0), because it is not necessary to remove the copper wire from the reaction. The proposed mechanism for photoinduced ATRP is shown in Scheme 2. This mechanism is a hybrid of ICAR ATRP and ARGET ATRP. Because radiation induces the reduction of X-Cu(II)/L to Cu(I)/L, the mechanism resembles ARGET ATRP. However, a halogen radical is formed, which resembles the generation of radicals in ICAR ATRP37. Scheme 2Mechanism of Photoinduced ATRP. Mechanism of Photoinduced ATRP. The present study aims to synthesize and characterize the MA polymerization in the presence of the MOF@Cu. The polymerizations were induced thermally in the presence of the copper wire or by using a red LED. Also, the kinetics of the polymerization were presented and followed a SET-LRP-type reaction, as determined from GPC, UV-Vis, and1 H NMR characterizations. The percentage of the living chain was determined using1 H NMR. Emulsion polymerization was conducted using a red LED, and the resulting particles were analyzed via scanning electron microscopy (SEM). Also, in the case of light-induced solution polymerization, Cu nanoparticles were generated and characterized by BFTEM. MOF@Cu plays a single role as a cocatalyst and is reduced by the copper wire to produce Cu(I) ions necessary to activate the polymerization. Materials and methods Materials Methyl acrylate (MA) and methyl methacrylate (Sigma-Aldrich) were purified by vacuum distillation under reduced pressure in a stream of argon gas. Cu (0) wire with a diameter of 0.025 mm was obtained from Alfa Aesar. Tetrahydrofuran (THF) (Aldrich), dimethyl formamide (DMF) (Aldrich) were purified by distillation, 2,2’-bipyridine (BiPy) (Aldrich), N, N, N′, N′′, N′′-pentamethyldiethylenetriamine (PMDETA) (Aldrich), CuCl (Aldrich), methanol (Aldrich), diethyl ether (EtOEt) (Aldrich), ethyl α-bromoisobutyrate (EBiB) (Aldrich), Copper benzene-1,3,5-tricarboxylate, Cu-BTC MOF, HKUST-1, Basolite C300 (MOF@Cu) (Aldrich), and sodium dodecyl sulphate (Merck) were used as received. In the case of Basolite C300, the terminology used in this paper was MOF@Cu. Experiments Polymerization of MA in the presence of different concentrations of MOF@Cu and copper wire In a 10 mL glass vial, 4 mL (4.4 × 10− 2 mol) of MA was added, followed by 3 mL of DMF and different amounts of MOF@Cu, namely 0.001 g (1.65 × 10− 6 mol) (MOF 1@Cu), 0.002 g (3.3 × 10− 6 mol) (MOF 2@Cu), and 0.003 g (4.95 × 10− 6 mol) (MOF 3@Cu). A magnetic PTFE stirring bar, wrapped with 5 cm of copper wire, was subsequently added to the vial in the presence of 10 mmol PMDETA. The vial was bubbling with nitrogen for 10 min and then sealed with a silicon rubber septum. Afterward, 0.06 mL of EBiB (3 × 10− 4 mol) was injected into the vial, and the polymerization was allowed to proceed at 70 °C under stirring at 200 rpm. Samples were taken periodically under a nitrogen blanket for gravimetric and GPC analysis. To establish the conversion, the collected samples were precipitated in methanol, filtered, and dried under reduced pressure. Polymerization of MA in the presence of MOF 2@Cu and red light The reaction is presented as in 2.2.1, but using a red LED (40 W) instead of a copper wire. The processing of the samples has been identical to that described in Sect. 2.2.1. Chain extension of the poly (MA) with MMA obtained at points 2.2.1, 2.2.2 The polymer synthesis was performed in DMF using the modified poly MA as the starting material, as described in Sect. 2.2.1 and 2.2.2. Thus, 0.2 g of poly MA was dissolved in 5 mL DMF, and 2 mL (1.88 × 10− 2 mol) MMA was added. The mixture was subjected to nitrogen purging, after which 0.0003 g CuCl (3 × 10− 6 mol) and 0.0005 g BiPy (3.2 × 10− 6 mol) were added. The reaction vial was sealed and heated at 80 °C under stirring for 2 h. Then, the reaction mixture was precipitated in methanol, filtered, and dried under vacuum until a constant mass was achieved. Emulsion polymerization of MA in the presence of red LED In a 25 mL glass vial containing 10 mL of water, 0.02 g (6.93 × 10− 5 mol) sodium dodecyl sulfate was dissolved. After that, 4 mL (4.4 × 10− 2 mol) of MA was added, followed by 0.003 g (4.95 × 10− 6 mol) of MOF@Cu and 0.17 mL (10 mmol) of PMDETA. The mixture was purged with nitrogen. After that, 0.06 mL (3 × 10− 4 mol) of EBiB was injected into the vial, and the polymerization was allowed to proceed under a red LED with stirring at 200 rpm for 24 h. Characterization The molecular weights of the obtained polymers were analyzed using a PL-GPC 50 Integrated GPC/SEC System (Agilent Technologies) with a 1 mL/min THF flow rate and a column oven temperature of 40 °C, employing polystyrene as a standard and a refractive index detector. The GPC equipment was calibrated using polystyrene standards (molecular weights ranging from 162 to 10 000 000 g/mol, in 18 points). Two types of columns have been used: MIXED-C: Range: 200 − 106 g/mol and Low Molecular Weight (100–104 g/mol). The HNMR analyses were performed on a Bruker Advance III HD 600 MHz spectrometer (Bruker, Rheinstetten, Germany), with a resonance frequency of 600.12 MHz for the 1 H nucleus, equipped with a 5 mm multinuclear direct detection z-gradient probe head (BBI). Samples were analyzed using CDCl3 as a solvent. The UV-VIS spectra were recorded on a UV-VIS-NIR spectrophotometer (UV 3600, Shimadzu) equipped with a quartz cell having a 10 mm light path. The synthesis protocol used was the same as presented in 2.2.1. section (MOF 1@Cu). Bright-field (BFTEM) Transmission Electron Microscopy images were acquired using an aberration-corrected 80–200 kV Titan Themis transmission electron microscope (Thermo Fisher Scientific, USA), operating at an accelerating voltage of 200 kV. Sample preparation involved placing a small amount of the dried material onto a 400-mesh holey coated Ni grid. Ni grid was chosen due to the nature of the particles. EDS analysis was also performed in STEM (scanning transmission electron microscopy) mode on a single particle to see the composition. The morphology of the polymer was analyzed using scanning electron microscopy (SEM) with a Nova NanoSEM 630 instrument (FEI Company, Hillsboro, OR, USA) at an acceleration voltage of 10 kV.The samples’ hydrodynamic diameter and surface charge were analyzed using a Beckman Coulter Delsa™Nano C instrument, employing dynamic light scattering (DLS) and electrophoretic light scattering (ELS), respectively. A dual 30 mW laser diode was used to illuminate the particles, generating time-dependent fluctuations in light intensity. For size determination, scattered light was detected at an angle of 165°, while zeta potential measurements were conducted at 15°, using appropriately diluted samples. A highly sensitive detector captured the scattered light signals. Data were processed using Delsa™Nano software version 3.73. Before measurement, the sample was diluted with deionized water at a 1:5 volume ratio (polymer dispersion: deionized water) and subjected to ultrasonication for 10 min to ensure proper dispersion. All measurements were conducted at room temperature, with each sample analyzed in triplicate. The samples’ hydrodynamic diameter and surface charge were analyzed using a Beckman Coulter Delsa™Nano C instrument, employing dynamic light scattering (DLS) and electrophoretic light scattering (ELS), respectively. A dual 30 mW laser diode was used to illuminate the particles, generating time-dependent fluctuations in light intensity. For size determination, scattered light was detected at an angle of 165°, while zeta potential measurements were conducted at 15°, using appropriately diluted samples. A highly sensitive detector captured the scattered light signals. Data were processed using Delsa™Nano software version 3.73. Before measurement, the sample was diluted with deionized water at a 1:5 volume ratio (polymer dispersion: deionized water) and subjected to ultrasonication for 10 min to ensure proper dispersion. All measurements were conducted at room temperature, with each sample analyzed in triplicate. X-ray diffraction (XRD) patterns were recorded using a 9 kW Rigaku SmartLab diffractometer (Osaka, Japan), equipped with a CuKα1 source that provides a monochromatic wavelength, λ = 0.15406 nm. During the measurements of the powder sample, the scan was initiated in θ/2θ mode (i.e., the source and detector arms are coupled). For the other samples, on glass, a grazing-incidence XRD configuration was employed, for which the incidence angle of the source was kept constant at 0.5˚ to remove the signal from the glass substrate. In both configurations, the scan step was 0.01˚/min, while the speed was set as 8˚/min. Results and Discussions To highlight the controlled character of the polymerizations in the presence of MOF@Cu, it must fulfill three conditions5,41,42: The increase in the polymer molecular weight with the conversion;Narrow values of the polydispersity indexes < 1.5;The possibility of block-copolymer synthesis. The increase in the polymer molecular weight with the conversion; The increase in the polymer molecular weight with the conversion; Narrow values of the polydispersity indexes < 1.5; Narrow values of the polydispersity indexes < 1.5; The possibility of block-copolymer synthesis. The possibility of block-copolymer synthesis. The first step in our research is a kinetic study of MA polymerization in the presence of network-like structures at different concentrations (MOF 1@Cu (1.65 × 10− 6 mol), MOF 2@Cu (3.3 × 10− 6 mol), and MOF 3@Cu (4.95 × 10− 6 mol). Figure 1 presents the variation of conversion and ln([M]0/[M]) as a function of reaction time. Fig. 1The dependence of conversion and ln([M]0/[M]) versus time for the polymerization of MA in the presence of different concentrations of MOF@Cu [MA]/[EBiB]/[MOF 1@Cu]/[PMDETA] = 178/1/0.000025/0.05 [MA]/[EBiB]/[MOF 2@Cu]/[PMDETA] = 178/1/0.000050/0.05 [MA]/[EBiB]/[MOF 3@Cu]/[PMDETA] = 178/1/0.000075/0.05 The dependence of conversion and ln([M]0/[M]) versus time for the polymerization of MA in the presence of different concentrations of MOF@Cu [MA]/[EBiB]/[MOF 1@Cu]/[PMDETA] = 178/1/0.000025/0.05 [MA]/[EBiB]/[MOF 2@Cu]/[PMDETA] = 178/1/0.000050/0.05 [MA]/[EBiB]/[MOF 3@Cu]/[PMDETA] = 178/1/0.000075/0.05 As shown in Fig. 1, the conversion values increase as the MOF@Cu concentrations decrease. Meanwhile, the conversion for MOF 1@Cu is higher than that for MOF 2@Cu, and for MOF 3@Cu is lower. The linear relationship of ln (M0/M) versus time provides initial evidence of controlled polymerization in all cases. To emphasize the controlled nature of the polymerization, Fig. 2 shows how molecular weight and polydispersity index depend on conversion. The polydispersity index values range from 1.2 to 1.48. Additionally, molecular weight increases as conversion progresses. Regarding the molecular weight dependence on conversion, two zones are observed: one with Mn values higher than the theoretical ones (slow initiation)43, and the second with smaller values (irreversible transfer)44. This different behavior could be explained by the different concentration of MOF@Cu used. The slow initiation is described by the failure to initiate all the monomer molecules. Irreversible transfer is possible due to the loss of equilibrium between copper species. Probably, Cu(0) concentration is much higher than that of Cu (II) provided by the MOF@Cu, maybe due to the high reaction rate. In this context, for the MOF 1@Cu system, control of polymerization is lacking. Also, Fig. 3 presents the GPC traces for the sample from all polymerizations. Fig. 2Molecular weights and polydispersity indexes dependence on the conversion and the average initiator efficiency values [MA]/[EBiB]/[MOF 1@Cu]/[PMDETA] = 178/1/0.000025/0.05 [MA]/[EBiB]/[MOF 2@Cu]/[PMDETA] = 178/1/0.000050/0.05 [MA]/[EBiB]/[MOF 3@Cu]/[PMDETA] = 178/1/0.000075/0.05 Molecular weights and polydispersity indexes dependence on the conversion and the average initiator efficiency values [MA]/[EBiB]/[MOF 1@Cu]/[PMDETA] = 178/1/0.000025/0.05 [MA]/[EBiB]/[MOF 2@Cu]/[PMDETA] = 178/1/0.000050/0.05 [MA]/[EBiB]/[MOF 3@Cu]/[PMDETA] = 178/1/0.000075/0.05 Fig. 3GPC traces for MOF 1@Cu (a); MOF 2@Cu (b) and MOF 3@Cu (c). GPC traces for MOF 1@Cu (a); MOF 2@Cu (b) and MOF 3@Cu (c). In the tables (Table S1-Table S3), the results of the polymerization in the presence of different concentrations of MOF@Cu are summarized. Analyzing the above data, the most controlled polymerization is observed for the MOF 2@Cu concentration. To support controlled polymerization, the next step was to synthesize a block copolymer using MOF 2@Cu (Sample 6) (Fig. 4). The block copolymer synthesis was activated using the system CuCl + BiPy ligand, which forms a soluble, well-defined Cu(I)/Cu(II) redox couple that efficiently45 performs atom-transfer activation and deactivation. Copper wire cannot satisfy this requirement due to its metallic state as Cu(0) and limited solubility, resulting in a slow conversion to Cu(I) through surface-mediated redox processes. Thus, the chain extension was performed with MMA, yielding Mn = 19 173 g/mol and Đ = 1.48. Fig. 4GPC traces for the block copolymer provided from sample 6-MOF 2@Cu. GPC traces for the block copolymer provided from sample 6-MOF 2@Cu. Considering the above results, it is essential to confirm that the polymerization in the presence of MOF 2@Cu is controlled. To highlight the proposed mechanism involved (which could be SET-LRP or SARA-ATRP), the polymerization was performed in a UV-Vis cuvette, and the protocol is the same as presented in Sect. 2.2.1., (MOF 2@Cu). The results are shown in Fig. 5, and it is easy to observe the accumulation of Cu(II) ions (wavelength 700 nm) with the increase in the reaction time46. The findings suggest a SET-LRP polymerization according to Virgil Percec’s studies28,29,47,48. Fig. 5UV-Vis spectra of the reaction and the accumulation of Cu (II) ions. UV-Vis spectra of the reaction and the accumulation of Cu (II) ions. by disproportionation. To emphasize the SET-LRP polymerization, the next step includes characterizing the polymerization using ¹H NMR. SET-LRP involves heterogeneous outer-sphere electron transfer (OSET) by nascent Cu(0), leading to faster activation of alkyl halides, a higher concentration of active radicals, and, consequently, more radical coupling and termination (Fig. 6). The percentage of the chain end functionality (26%) and molecular weight (9 764 g/mol) were calculated according to49. Thus, in the case of SET-LRP, a higher concentration of active radicals leads to a significantly greater rate of radical coupling and bimolecular termination. The spectrum obtained from PMA (Fig. 6), prepared in DMF, matches the spectrum of PMA prepared in DMSO49. The resonance of methyl protons from the ester group of the repetitive units is assigned at 3.65 ppm, while the ones from the terminal bromo chain-end are at 3.77 ppm. The signal of the methyl protons of the OCH2CH3 group is at 1.24 ppm. The low intensity signal at 4.24 ppm corresponds to the -CH-Br of the active terminal bromo chain-end. The percentage of the chain end functionality (26%) was determined by considering the following ratio50: \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\rm Chain \:end \:functionality \:\%}=\:\frac{I(H-10)}{I(H-6;H-{6}^{{\prime\:}})/6}\times\:100$$\end{document} -where I(H10) is the integral of the PMA terminal bromo chain-end at δ = 4.24 ppm and I(H-6; H-6’) is the integral of the -C(CH3)2 from the initiator fragment at δ = 1.13 ppm. Additionally, the pMA-Br molecular weight was calculated using the Eq. 50: \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\rm Mn}^{NMR}=\:\left[\frac{\mathrm{I}\:\left(\mathrm{H}-8\right)}{\frac{\mathrm{I}\left(H-6;\mathrm{H}-{6}^{{\prime\:}}\right)}{6}}+1\right]\times\:{\rm Mw_{MA}+Mw_{EBiB}}^{50}$$\end{document} -where I(H-8) is the integral of the pMA main chain -CH2-CH-CH2 proton at δ = 2.30 ppm and I(H-6;H-6’) is the integral of the -C(CH3)2 from the initiator fragment at δ = 1.13 ppm. Tacticity measurement was made by calculating the ratio raceme: meso (H-7r/H-7 m) and was found to be 112.39:100.5350. Thus, it can be concluded that MOF@Cu plays at least a cocatalyst role. For the second involvement as a ligand (dual role), the polymerizations were conducted in the absence of PMDETA. Unfortunately, the reactions don’t initiate, so they play a single role as a cocatalyst. Fig. 6¹H NMR spectrum of PMA (Sample 3- Table 2). ¹H NMR spectrum of PMA (Sample 3- Table 2). (prepared in deuterated DMSO-d6). The ¹H NMR spectrum of the block copolymer (Figure S1) exhibits the characteristic resonances of the α‑methyl protons at 0.94, 0.75, and 0.47 ppm52. In comparison with the PMA homopolymer, the emergence of these signals unambiguously confirms the successful formation of the targeted block copolymer. To elucidate the synthesis of the nanomaterials, X‑ray diffraction (XRD) patterns were collected for pristine Cu@MOF and sample 6 (MOF2@Cu). The diffraction profile of Cu@MOF exhibits the characteristic reflections expected for this material, confirming the phase purity of the framework53. In the nanocomposite, the crystalline features of the MOF coexist with an amorphous contribution provided by the polymer. Several reflections attributable to the parent MOF are retained in the composite, further supporting the successful formation of a hybrid material54,55. Fig. 7XRD patterns of the pristine MOF@Cu (1) and the hybrid materials (2). XRD patterns of the pristine MOF@Cu (1) and the hybrid materials (2). Considering the controlled polymerization of the MOF 2@Cu system, another direction is to synthesize the polymer in the presence of a red LED but in the absence of a copper wire. The reduction of the Cu (II) ions is realized by the tertiary amine. Under red LED irradiation, Cu (II)* excited state is produced. Cu (I) ions could activate the polymerization. The proposed mechanism is presented in Scheme 356. Scheme 3The proposed mechanism of photopolymerization. The proposed mechanism of photopolymerization. Comparing conventional polymerization (in the presence of a copper wire) with photopolymerization (Fig. 8a), it can be observed that conventional polymerization is faster. The explanation may lie in the lower concentration of radical species obtained during photopolymerization. Figure 8b presents the GPC traces for the samples belonging to the photopolymerization, specifically for the chain-end fidelity (block copolymer). Table 4 summarizes the results. Also, the molecular weight increases with conversion, and the polydispersity indices are in good agreement with ATRP theory. Fig. 8Comparative conversion for the conventional polymerization and for the polymerization in the presence of red LED, and the GPC traces for the polymers obtained in the presence of the LED ([MA]/[EBiB]/[MOF 2@Cu]/[PMDETA] = 178/1/0.000050/0.05). Comparative conversion for the conventional polymerization and for the polymerization in the presence of red LED, and the GPC traces for the polymers obtained in the presence of the LED ([MA]/[EBiB]/[MOF 2@Cu]/[PMDETA] = 178/1/0.000050/0.05). Table 4Photopolymerization results for MOF 2@Cu*.SampleTime (min)Conv.(%)Mn, GPC(g·mol− 1)ĐMn, theo(g/mol)Ieff (%) Sample 1 302.1135001.403239.22 Sample 2 608.9642001.40137232.65 Sample 3 12017.2047421.43263355.52 Sample 4 18022.0351401.40337365.61 Sample 5 24025.5757001.35391568.67 Block-copolymer 1808515 0591.39-*[MA]/[EBiB]/[MOF 2@Cu]/[PMDETA] = 178/1/0.000050/0.05.Initiation efficiency (I) = Mn, theo/Mn, GPC. Table 4Photopolymerization results for MOF 2@Cu*.SampleTime (min)Conv.(%)Mn, GPC(g·mol− 1)ĐMn, theo(g/mol)Ieff (%) Sample 1 302.1135001.403239.22 Sample 2 608.9642001.40137232.65 Sample 3 12017.2047421.43263355.52 Sample 4 18022.0351401.40337365.61 Sample 5 24025.5757001.35391568.67 Block-copolymer 1808515 0591.39-*[MA]/[EBiB]/[MOF 2@Cu]/[PMDETA] = 178/1/0.000050/0.05.Initiation efficiency (I) = Mn, theo/Mn, GPC. Photopolymerization results for MOF 2@Cu*. *[MA]/[EBiB]/[MOF 2@Cu]/[PMDETA] = 178/1/0.000050/0.05. Initiation efficiency (I) = Mn, theo/Mn, GPC. To evaluate the chain‑end functionality, a ¹H NMR spectrum was recorded (Figure S2), yielding a value of 98%. When compared with the polymerization conducted in the presence of copper wire, the higher conversion attained and it is accompanied by an increased extent of bimolecular termination, both processes being further promoted by the elevated reaction temperature. Photo-induced reaction can often be conducted at or near ambient temperatures, which minimizes thermally driven side reactions, chain transfer, and irreversible bimolecular termination57. Moreover, the polymerizations displayed temporal control behavior in response to light-on/off change cycles (Fig. 9). In the absence of the LED, the conversions are limited. These results demonstrate the efficient nature of the MOF 2@Cu catalyst in achieving well-controlled characteristics through temporal control of the polymerization. Fig. 9Light–on–off experiments for MOF 2@Cu. Light–on–off experiments for MOF 2@Cu. [MA]/[EBiB]/[MOF 2@Cu]/[PMDETA] = 178/1/0.000050/0.05. As can be observed in Fig. 9, the polymerization reaction exhibits a yellow color, characteristic of copper nanoparticles58. The first method of characterization consists of measuring the sample’s UV-Vis absorbance at the end of polymerization under LED illumination. As shown in Fig. 10, the characteristic wavelength is situated around 300 nm, as is typical for nanoparticles59. Fig. 10UV-Vis absorbance for copper particles. UV-Vis absorbance for copper particles. BFTEM images (Fig. 11) reveal spherical particles, approximately 200 nm in size, amorphous, and uniformly distributed. EDS analysis confirms that the particles are composed of Cu. Ni is also present and comes from the support grid. The EDS spectra were obtained only from the particles that are in the red square. Fig. 11BFTEM and STEM images of the sample at the end of polymerization. BFTEM and STEM images of the sample at the end of polymerization. initiated by a red LED. As a direct application of red LED-induced polymerization, an emulsion was obtained with a conversion of 90%, as presented in Fig. 12. The mean diameters of the particles are around 230 nm. To confirm the controlled characteristics of polymerization, GPC analysis was also performed. The molecular weight obtained was 574 200 g/mol, with Đ = 1.4. Because SEM provides only localized surface information, dynamic light scattering (DLS) measurements were conducted to obtain a statistically representative assessment of the dispersion. As shown in Fig. 12d, the particles exhibit an average hydrodynamic diameter of approximately 250 nm. The emulsion displays good colloidal stability, as indicated by the zeta potential value of − 28.56 mV, which is sufficiently negative to ensure electrostatic repulsion between particles. Also, by 1H NMR (Figure S3), the chain end functionality was estimated to be around 67%. This value is consistent with the sequence of physicochemical processes occurring in the system—namely nucleation, monomer diffusion, and particle growth—which collectively govern the chain‑end fidelity60. Fig. 12SEM (a and b), GPC results (c), and DLS (d) of the emulsion initiated by the red LED. [MA]/[EBiB]/[MOF 2@Cu]/[PMDETA] = 178/1/0.000075/0.05. SEM (a and b), GPC results (c), and DLS (d) of the emulsion initiated by the red LED. [MA]/[EBiB]/[MOF 2@Cu]/[PMDETA] = 178/1/0.000075/0.05. Conclusions The present study, for the first time in the specific literature, shows the polymerization of MA in the presence of MOF@Cu, using copper wire or a red LED as a cocatalyst. In the case of copper wire, the kinetics exhibit controlled polymerization, as evidenced by the linear dependence of molecular weights on conversion, narrow polymerization indices, and the possibility of block copolymer synthesis. The characterizations were made using GPC, UV-Vis, 1H NMR. In the case of the red LED, polymerization proceeds more slowly than with copper wire, and LED-based temporal control of the reaction was demonstrated. In this case, copper particles with a diameter of around 250 nm were generated and characterized by BFTEM and UV-Vis. As a practical application of polymerization initiated by a red LED, an emulsion has been obtained with Mn = 574 200 g/mol and Đ = 1.4. Supplementary Information Below is the link to the electronic supplementary material. Supplementary Material 1 Supplementary Material 1