Comparative study of TiO2 and graphene oxide enhancement of the removal of methylene blue dye using PVA/PEO hydrogels synthesized by gamma irradiation Authors: Mai M. Mohamed, Asmaa Sayed, Dalia E. Hegazy Published: 2026 ABSTRACT Water pollution from industrial effluents, particularly textile dyes, represents a significant environmental challenge. In this study, polyvinyl alcohol (PVA)/polyethylene oxide (PEO)/poly(acrylic acid) (PAAc) hydrogels were synthesized via gamma irradiation (30 kGy) and modified with titanium dioxide (TiO₂) and graphene oxide (GO) nanoparticles to enhance methylene blue (MB) dye removal. Comprehensive characterization using FTIR, XRD, AFM, SEM, and TGA confirmed the successful incorporation of the nanofillers and their influence on the structural and physicochemical properties of the hydrogels. The addition of TiO₂ and GO significantly improved the gel fraction from 65% (neat hydrogel) to 99% and 98%, respectively. Swelling behavior showed a pH-dependent response, with maximum swelling observed at pH 10 after 24 h, following the order: PVA/PEO/PAAc < PVA/PEO/PAAc/TiO₂ < PVA/PEO/PAAc/GO. Batch adsorption experiments were conducted under controlled conditions (pH 10, adsorbent dosage 0.1 g, initial MB concentration 20 mg/L, and contact time 24 h). The removal efficiencies reached 64%, 98%, and ~ 100% for PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂, and PVA/PEO/PAAc/GO, respectively. Adsorption kinetics were better described by the pseudo-first-order model, indicating that physisorption plays a dominant role in the rate-controlling step. Isotherm analysis showed good agreement with the Langmuir model, suggesting predominantly monolayer adsorption on relatively homogeneous surfaces. Overall, both TiO₂- and GO-reinforced hydrogels exhibited enhanced adsorption performance compared to the neat hydrogel. The superior performance of GO-based hydrogels is attributed to their higher surface area and abundance of oxygen-containing functional groups, which facilitate dye–adsorbent interactions. These findings demonstrate the potential of radiation-synthesized nanocomposite hydrogels as efficient materials for dye removal, while further studies are required to evaluate their performance under realistic wastewater conditions. Introduction Organic dyes are among the most polluted species that discharged into water as effluents of many industries such as tanning, painting, ceramics and electronics [1, 2]. The most determinative effect of dyes to environment is that they prevent the sunlight from passing deep into aquatic flora and Fauna and cause significant depletion in the green coverage layer [3]. Moreover, they are highly harmful to human health and can induce several acute diseases [4–6]. Due to their high water solubility and ease of interaction with negatively charged cell membrane surfaces, cationic dyes, such as Methylene blue, are more hazardous than anionic dyes and concentrate in the cytoplasm of cells [7]. Several methodologies are applied to eliminate dyes from aqueous solutions. They include chemical oxidation [8], photocatalytic degradation [9, 10], precipitation and coagulation [11], membrane techniques [12], biological treatment [13]and adsorption onto different sorbents [14–17].Generally, treatment by adsorption finds strong potential over other methods due to ease of application, abundancy of different sorbents, recyclability of sorbents and generation of no wastes or toxic materials [18, 19] . On the other hand, hydrogel sorbents are being superior over other sorbents due to their great ability of absorbing and retaining huge amounts of adsorbates [20, 21]. Hydrophilic polymers are cross-linked chemically and/or physically to form hydrogels, three-dimensional networks with improved absorption and retention capabilities [22, 23]. They have ionic functional groups, allowing them to absorb and retain ionic dyes from wastewaters, like MB. Recently, hydrogel nanocomposites are used in wastewater treatment for enhanced adsorption due to their ability to modify the physical and catalytic properties of nanocomposite by tuned the materials with tailored properties such as large surface area resulted from incorporation of nanoparticles inside hydrogel matrix [24], reactivity and morphology. Hydrogels are generally made from natural polymers or green polymer. Poly (vinyl alcohol) is a green polymer with pronounced importance in different fields, such as packaging [25, 26], pharmaceutical [27, 28] and industrial applications [29, 30]. In wastewater treatment, Poly (vinyl alcohol) has been combined with other constituents to give rise up excellent formulations for removal of different pollutants [31, 32]. In this regard, PVA/ Arabic gum hydrogels were prepared via gamma irradiation for removal of heavy metals from wastewater [33].Qudah et al. prepared some crosslinked poly(vinyl alcohol)-based hydrogels for removal of heavy metals from simulated solutions [34]. Additionally, by using gamma-induced radiation polymerization, poly (acrylic, polyvinyl alcohol) copolymer hydrogels with different PVA (polyvinyl alcohol) contents were created. This mixture was applied to the purifying of water [35]. However, combination of poly (vinyl alcohol) hydrogels with carbonaceous and inorganic materials into composite formulations for wastewater treatment application is considered a recent approach. Under visible light illumination, Liu et al. used an Axylan/PVA/TiO2 hybrid material as a photocatalyst for the photocatalytic decolorization of Astrazon brilliant red-4G and ethyl-violet dyes [36], Alireza et al. enhanced photocatalytic efficiency of 81.47% for oxytetracycline degradation (OTC) using gray-shaded titania. This modified titania demonstrated better visible-light photocatalytic activity compared to pristine P25, attaining 81.47% degradation efficiency during degradation tests [37]. In another work, SDS/PVA/ZnO hydrogel composite was used as an active catalyst for the photodegradation of reactive red azo dye [38]. Zinc oxide (ZnO) particle-loaded polyvinyl alcohol/cellulose nanofibril (PVA-CNF) aerogel nanocomposites were created, according to [39].Methylene blue (MB) was sequestered in aqueous solution using the aerogels through immediate adsorption and catalytic breakdown with sodium borohydride. On the other hand, a special type of water-soluble, aerobically biodegradable thermoplastics is called poly (ethylene oxide, or PEO). PVA’s main hydroxyl group has the potential to create a hydrogen bond with PEO’s ether oxygen [40]. Because acrylic acid can absorb more than five to ten times its weight in water, it was added because it is the foundation of a class of substances known as super absorbents [41]. The addition of AAc enhanced the polymer’s ionizable groups. In order to increase the interaction between the cationic groups of MB dye and the functionalities of adsorbents, nanocomposites comprise a lot of carboxyl groups [42]. One of the most likely functional adsorption materials that can now be used to clean many different sorts of contaminated water sources is graphene-based hydrogels [43]. Due to its low cost of mass production, great water dispersibility, high surface area, and strong adsorption capacity, Graphene oxide (GO) is currently one of the most often used inorganic cores in composite synthesis. GO is typically a two-dimensional, one atom thick carbonaceous substance. It has many hydroxyl, epoxy, carbonyl, and carboxyl COOH groups, as well as other hydrophilic oxygenated functional groups. These compounds increase GO’s miscibility with the polymer matrix and make it hydrophilic [44]. Titanium dioxide (TiO2) plays a predominant role in polymeric hydrogel synthesis due to its non-toxicity, low cost and inert chemical properties and can be used in removing several types of organic poll. The electron rich Titanium dioxide and Graphene oxide capable of interacting with copolymer containing acrylate carbonyl group [45], so enhancing the polymer properties and introducing high surface area to improve the adsorption process. Therefore, a new combination between the previously mentioned candidates is introduced as effective sorbents for MB dye. In this contest, the preparation of Poly vinylalcohol ( PVA) /Polyethylene oxide(PEO) /Polyacrylic acid (PAAc) hydrogels reinforced separately with Titanium dioxide (TiO₂) and Graphene oxide (GO) nanoparticles using gamma irradiation is discussed. Gamma radiation is an effective facile technique for inducing crosslinking by generating numerous radical species, such as hydroxyl (•OH) and hydrogen (•H) radicals. Following their attacking on the polymer chains, these radicals generate a number of polymer macroradicals that take part in both intra- and intermolecular free-radical recombination operations [46]. Finally, a stable crosslinked polymeric network was produced [47].The prepared polymeric formulations were characterized by FTIR, XRD and AFM analyses and their adsorption capacity towards methylene blue dye was verified under different operating conditions. Materials and experiment Materials Acrylic acid (C3H4O2) AAc stabilized with 200 ppm MEHQ 99.55%, purchased from ACROS ORGANICS, New Jersy, USA. Poly (vinyl alcohol) (C2H4O)n PVA, purchased from BLULUX Laboratories (p) Ltd., INDIA, M.W. app. 14,000 LR [Laboratory Rasayan s.d.finf-chem Ltd, Boisar 401501]. Polyethylene oxide (PEO) Mw 400.000 was purchased from Sigma-Aldrich Co. Methylene bisacrylamide MBAM was purchased from Oxford Laboratory Reagent, India, as an AR. Titanium dioxide TiO2 (nano-powder) was obtained from Sigma-Aldrich Co. with an average particle size of 21 nm. Graphene oxide (GO) was purchased from Qualikems Laboratory Reagent India (average size 1–3 μm and thickness 1–5 nm). A Cationic dye was used as a model for application: Methylene blue (MB) C25H30ClN3, M.W. = 407.99, purchased from Qualikems Fine Chemicals Pvt. Ltd., New Delhi − 110 060, absorption max = 663 nm. All chemicals were used as received without further purification. Irradiation of the samples was carried out using a 60Co gamma source in Egypt, with an average dose rate of 2.70 kGy/h and a total dose of 30 kGy, which is adequate for preparing a stable hydrogel. Preparation of PVA/PEO/PAAc/TiO2 and PVA/PEO/PAAc/GO Nanocomposite hydrogels A Simple preparation method was applied. First,1 g of PVA was dissolved in 50 ml of distilled water under continuous stirring at 70 °C for 2 h, while 1 g of PEO was dissolved in 50 ml of distilled water. The two solutions were then mixed. Subsequently, 7.5 ml of AAc was added to the PVA/PEO solution, and the mixture was stirred until a completely homogeneous solution was obtained. A high percentage of vinyl monomers in the copolymer solution may lead to the formation of a three-dimensional crosslinked hydrogel [48]. Methylene bisacrylamide (MBAM; 0.5 g) was added to the prepared polymer solution to enhance crosslinking; the total polymer concentration was adjusted to 9.5 wt%, and the solution was exposed to gamma irradiation at a total dose of 30 kGy. The swelled hydrogel with a gel fraction of approximately 65% was obtained. Nanocomposite hydrogels were prepared by adding different concentrations of TiO2 and GO (1,2,3 wt%) of the total polymer concentration of (9.5 wt %), and of composition 1:1:7.5 wt/wt of PVA: PEO: AAc in presence of 5.2% MBAM crosslinker. Ultrasonication was used during the preparation of nanocomposite hydrogels to ensure proper dispersion of the nanoparticles within the polymer matrix. The resulting solutions were poured into test tubes and irradiated with 60Co gamma rays to a total dose of 30 kGy. After the irradiation process, the hydrogel obtained was removed from the test tubes, cut into regular small disks, and dried in an oven at 60 °C. The codes and the composition of the prepared nanocomposites are given in Table 1. Table 1The composition of hydrogel nanocomposites (wt/wt) of the total polymer concentration (9.5 wt%)CodePVA (g)PEO (g)AAc (mL)MBAM (g)TiO2 (wt%)GO (wt%)Irradiation dose 30 kGyPVA/PEO/PAAc117.50.500PVA/PEO/PAAc/TiO2a117.50.510PVA/PEO/PAAc/TiO2b117.50.520PVA/PEO/PAAc/TiO2c117.50.530PVA/PEO/PAAc/GOa117.50.501PVA/PEO/PAAc/GOb117.50.502PVA/PEO/PAAc/GOc117.50.503 Table 1The composition of hydrogel nanocomposites (wt/wt) of the total polymer concentration (9.5 wt%)CodePVA (g)PEO (g)AAc (mL)MBAM (g)TiO2 (wt%)GO (wt%)Irradiation dose 30 kGyPVA/PEO/PAAc117.50.500PVA/PEO/PAAc/TiO2a117.50.510PVA/PEO/PAAc/TiO2b117.50.520PVA/PEO/PAAc/TiO2c117.50.530PVA/PEO/PAAc/GOa117.50.501PVA/PEO/PAAc/GOb117.50.502PVA/PEO/PAAc/GOc117.50.503 The composition of hydrogel nanocomposites (wt/wt) of the total polymer concentration (9.5 wt%) Determination of gelation (%) (Gel%) and swelling % Hydrogel samples were precisely weighed (Wo), submerged in distilled water for 24 h, and then dried to achieve constant weight (Wd). The following Eq. (1) was used to calculate the gel%:1\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:Gel\:\left(\%\right)=\frac{{W}_{d}}{{W}_{0}}\times\:100$$\end{document} where Wd is the dried gel weight after extraction, and Wo is the dried gel weight before extraction. Swelling studies The prepared nanocomposite hydrogels were used to investigate swelling behavior as a function of pH, time, and nanoparticle concentration. Shortly after, Pre-weighed dried hydrogel discs were immersed in known volumes of distilled water. At predetermined time intervals, the samples were taken out of the solution and weighed after eliminating the extra surface water. The following calculation was used to compute the percent swelling (S %) [22]:2\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:S\:\left(\%\right)=\frac{{W}_{s}-{W}_{0}}{{W}_{0}}\times\:100\:\:$$\end{document} where: Ws is the weight of swollen hydrogel. Wo is the initial weight of dry hydrogel. Characterization Atomic Force Microscopy (AFM), the surface images of hydrogels were imaged using a Flexaxiom nanosurf with a non-contact mode using an NCLR rectangular shape cantilever with a frequency of 9 kHz. Fourier Transform Infrared Spectroscopy (FTIR) was used to study the functional group in the wave number range of 4000–400 cm-1 using a Bruker Vertex 70 FTIR spectrophotometer equipped with a HYPERION TM series microscope (Bruker Optic GmbH, Ettlingen, Germany) and an ATR unit for solid samples measurement were used in this study. X-ray diffraction measurements (XRD) were conducted at room temperature. XRD pattern (intensity vs. diffraction angle plate) was recorded in the range of diffraction angle 2θ = 10–80° at a scan speed of 8o/min using (XRD-6000) with Cu-target. Thermal gravimetric analysis (TGA), thermal stability of the prepared hydrogels was investigated using a Shimadzu-50 instrument (Kyoto, Japan) at a heating rate of 10 °C/min under flowing nitrogen (20 ml/min) from room temperature to 600 °C. Adsorption of methylene blue The adsorption of MB dye on PVA/PEO/PAAc/TiO2 (or GO) nanocomposite hydrogels was investigated by batch experiments, in which a definite weight of nanocomposite was immersed in 50mL of a dye solution. The effects of TiO2 content, GO content, pH, initial dye concentration, immersion time, and adsorbent weight on adsorption behavior were studied. The amount of dye remaining after a predetermined adsorption time was measured at λ = 663 nm using a UV-Vis Shimadzu 1700 spectrophotometer. The amount of MB adsorbed was calculated using Eq. (3) [48]:3\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{e}=\frac{({C}_{0}-{C}_{e})V}{W}\:\:\:$$\end{document} where w is the weight of the dried hydrogel sample (g), qe is the amount adsorbed per unit mass of the adsorbent (mg/g), Co and Ce are the concentrations of MB solution at the beginning and equilibrium (mg/L), and V is the volume of dye solution in L. Result and discussion Gel % and swelling (%) studies Various TiO₂ and GO nanoparticle concentrations (wt%) were incorporated into PVA/PEO/PAAc hydrogels via gamma irradiation at 30 kGy. The gelation and swelling behavior of the resulting nanocomposites were investigated as a function of nanoparticle content, pH, and time. Effect of nanoparticle concentration on gel% and swelling% Figure 1a and b illustrate the effect of different TiO₂ and GO concentrations on the gel content and swelling behavior of PVA/PEO/PAAc hydrogels, respectively. As the concentration of TiO₂ and GO increased, the gel % improved significantly from 65% up to 99.6% for TiO₂ and 97.3% for GO at 2 wt%. This increase is attributed to enhanced crosslinking density via covalent and hydrogen bonding between the polymer chains and nanoparticles. The swelling behavior in Fig. 1b shows that the addition of nanoparticles initially enhances the swelling percentage due to increased water diffusion facilitated by surface charges on TiO₂ and functional groups on GO. However, further increases in nanoparticle concentration (particularly at 2–3 wt%) led to a decline in swelling. In TiO₂-based hydrogels, this may be due to “strong knot tightening” effects resulting from chelation with hydroxyl groups, which restrict polymer chain expansion [49]. In the case of GO, excessive loading may lead to dense entanglements and strong interactions between GO sheets and the hydrogel network, thereby impeding water uptake [50]. Figure 1c presents the swelling response of PVA/PEO/PAAc hydrogels in buffer solutions across a pH range of 2 to 11. At acidic pH (2–6), the carboxylic acid groups remain protonated, allowing hydrogen bonding between –COOH and –OH groups, thereby reducing swelling [51]. At higher pH levels (9–10), deprotonation leads to ionization of –COOH to –COO⁻, causing strong electrostatic repulsion that expands the polymeric network [52].The swelling reaches a peak (1069%) at pH 10 Effect of pH on swelling behavior Fig. 1a Effect of TiO₂ and GO nanoparticle concentrations on Gel% of PVA/PEO/PAAc hydrogels. b Effect of TiO₂ and GO nanoparticle concentrations on equilibrium swelling% of PVA/PEO/PAAc hydrogels. c Swelling behavior of PVA/PEO/PAAc hydrogel at various pH values. d Swelling% of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂, and PVA/PEO/PAAc/GO hydrogels at pH 10 as a function of time. Further pH increase causes reduced swelling due to the screening effect from counter ions (e.g., Na⁺), which shield the charges and diminish repulsive forces [52] a Effect of TiO₂ and GO nanoparticle concentrations on Gel% of PVA/PEO/PAAc hydrogels. b Effect of TiO₂ and GO nanoparticle concentrations on equilibrium swelling% of PVA/PEO/PAAc hydrogels. c Swelling behavior of PVA/PEO/PAAc hydrogel at various pH values. d Swelling% of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂, and PVA/PEO/PAAc/GO hydrogels at pH 10 as a function of time. Further pH increase causes reduced swelling due to the screening effect from counter ions (e.g., Na⁺), which shield the charges and diminish repulsive forces [52] Swelling kinetics as a function of time The time-dependent swelling behavior of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂a (1 wt%), and PVA/PEO/PAAc/GOb (2 wt%) hydrogels at pH 10 is shown in Fig. 1d. All samples exhibited rapid swelling during the first 6 h, followed by a gradual approach to equilibrium by 24 h. The swelling trend followed the order: PVA/PEO/PAAc < PVA/PEO/PAAc/TiO₂a < PVA/PEO/PAAc/GOb, indicating that GO imparts a superior water-uptake capacity due to its abundant oxygen-containing functional groups [53]. Overall, the incorporation of both TiO₂ and GO nanoparticles significantly enhanced the gelation and swelling behavior of PVA/PEO/PAAc hydrogels; however, GO demonstrated superior swelling capacity and responsiveness. This can be attributed to the high surface area and rich oxygen-containing functional groups on GO, which promote stronger interactions with the hydrogel network and greater water uptake [54]. In contrast, TiO₂ contributed more effectively to increasing gel%, likely due to its ability to reinforce the crosslinked structure [55]. These differences suggest that GO-based hydrogels may be more advantageous for dye adsorption applications due to their higher swelling capacity, whereas TiO₂-based hydrogels offer enhanced structural stability. Surface morphology and topography Atomic force microscopy (AFM) Atomic Force Microscopy (AFM) provides high-resolution three-dimensional surface topography and is widely employed to characterize the morphological features of hydrogel materials. It enables the evaluation of key surface parameters such as height (Z-axis), surface roughness (Ra), and texture evolution, which are essential for understanding structural changes within the hydrogel network [56–58]. AFM images of the dry hydrogels and their corresponding methylene blue (MB)-loaded samples are presented in Fig. 2, with the associated quantitative data summarized in Table 2. The neat PVA/PEO/PAAc hydrogel exhibited a relatively rough surface (Ra = 8.794 nm), indicating heterogeneous polymer distribution and surface irregularities. Following MB adsorption, the surface roughness decreased to 3.316 nm, accompanied by a slight increase in surface height, suggesting surface coverage by dye molecules and partial smoothing of surface features. The TiO₂-containing hydrogel displayed a smoother initial surface (Ra = 3.235 nm), reflecting uniform nanoparticle dispersion within the hydrogel matrix; after adsorption, the roughness further decreased to 1.214 nm, while the surface height increased significantly, indicating morphological changes associated with dye accumulation on the surface. In contrast, the GO-loaded hydrogel exhibited higher initial roughness (Ra = 7.22 nm), likely due to the layered structure and partial stacking of graphene oxide sheets. After MB adsorption, the roughness decreased to 2.189 nm, with a notable increase in surface height, indicating surface modification following interaction with dye molecules. The consistent reduction in surface roughness across all samples suggests effective surface coverage by MB; however, since AFM measurements were conducted on dry samples, the observed changes are limited to surface topography and cannot be used to directly infer adsorption mechanisms, multilayer formation, or adsorption capacity. Overall, the AFM results demonstrate that nanoparticle incorporation modifies the surface morphology of the hydrogels, and the differences observed between TiO₂- and GO-containing systems reflect variations in surface structure and texture that may influence adsorption behavior, as discussed in subsequent sections. Table 2AFM data of PVA/PEO/PAAc hydrogel, PVA/PEO/PAAc/TiO2a, and PVA/PEO/PAAc/GOb nanocomposite hydrogels before and after MB dye adsorptionNo.CodeHeight (nm)Scale (nm)Data analysisRa(nm) (average area roughness)1-PVA/PEO/PAAc10.8313 × 313Line fit8.7942-PVA/PEO/PAAcMB17.3313 × 313Line fit3.3163-PVA/PEO/PAAc/TiO2a3.93313 × 313Line fit3.2354-PVA/PEO/PAAc/TiO2aMB83313 × 313Line fit1.2145-PVA/PEO/PAAc/GOb43.5313 × 313Line fit7.226-PVA/PEO/PAAc/GObMB184313 × 313Line fit2.189 Table 2AFM data of PVA/PEO/PAAc hydrogel, PVA/PEO/PAAc/TiO2a, and PVA/PEO/PAAc/GOb nanocomposite hydrogels before and after MB dye adsorptionNo.CodeHeight (nm)Scale (nm)Data analysisRa(nm) (average area roughness)1-PVA/PEO/PAAc10.8313 × 313Line fit8.7942-PVA/PEO/PAAcMB17.3313 × 313Line fit3.3163-PVA/PEO/PAAc/TiO2a3.93313 × 313Line fit3.2354-PVA/PEO/PAAc/TiO2aMB83313 × 313Line fit1.2145-PVA/PEO/PAAc/GOb43.5313 × 313Line fit7.226-PVA/PEO/PAAc/GObMB184313 × 313Line fit2.189 AFM data of PVA/PEO/PAAc hydrogel, PVA/PEO/PAAc/TiO2a, and PVA/PEO/PAAc/GOb nanocomposite hydrogels before and after MB dye adsorption Fig. 2AFM of PVA/PEO/PAAc hydrogel, PVA/PEO/PAAc/TiO2a, and PVA/PEO/PAAc/GOb nanocomposite hydrogels before and after MB dye adsorption AFM of PVA/PEO/PAAc hydrogel, PVA/PEO/PAAc/TiO2a, and PVA/PEO/PAAc/GOb nanocomposite hydrogels before and after MB dye adsorption SEM investigation The surface morphology of the swelled hydrogels PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂a, and PVA/PEO/PAAc/GOb was examined using Scanning Electron Microscopy (SEM), and the micrographs are shown in Fig. 3. These images provide insight into the influence of nanoparticle incorporation on the hydrogel structure. Fig. 3SEM of PVA/PEO/PAAc hydrogel (a), PVA/PEO/PAAc/TiO2a (b), and PVA/PEO/PAAc/GOb (c) nanocomposite hydrogels, SEM of PVA/PEO/PAAc hydrogel (a), PVA/PEO/PAAc/TiO2a (b), and PVA/PEO/PAAc/GOb (c) nanocomposite hydrogels, The pristine PVA/PEO/PAAc hydrogel (Fig. 3a) exhibited a relatively smooth surface with uniformly distributed pores, indicating a highly porous structure that favors water uptake and swelling. Upon incorporation of TiO₂ nanoparticles (Fig. 3b), the surface structure became notably denser and more compact. The pores observed in the native hydrogel largely disappeared, and the surface exhibited an irregular texture. This transformation suggests strong interactions between TiO₂ and the polymer matrix, thereby enhancing crosslinking density and reducing porosity. These changes are consistent with the reduced swelling and the improved gel fraction observed in TiO₂-containing hydrogels. In contrast, the GO-loaded hydrogel (Fig. 3c) retained visible small pores and a more textured surface compared to the TiO₂-based sample. The morphology suggests that GO incorporation helps maintain micro-porosity while simultaneously reinforcing the network. This supports the observed enhancement in swelling and dye uptake, driven by GO’s functional groups and layered structure. The SEM and AFM analyses together provide a comprehensive picture of the morphological and structural impact of TiO₂ and GO nanoparticles on the hydrogel matrix. SEM revealed that TiO₂ incorporation leads to a denser, pore-suppressed surface, while AFM confirmed lower height and surface roughness, indicating reduced porosity and tighter network compaction. Conversely, GO incorporation preserved surface pores in SEM and increased surface height and roughness in AFM, supporting the presence of a more open, layered, and functionalized network structure. These findings reinforce that TiO₂-based hydrogels favor structural stability and crosslink density, whereas GO-based hydrogels promote higher swelling, porosity, and dye removal capacity. FTIR analysis Fourier Transform Infrared (FTIR) spectroscopy was employed to investigate the structural interactions between the polymer components and the incorporated nanoparticles, particularly in terms of hydrogen bonding and possible complexation. The FTIR spectra of the prepared hydrogels are presented in Fig. 4. The spectrum of the PVA/PEO/PAAc hydrogel exhibits characteristic absorption bands corresponding to its constituent polymers. A broad band centered at approximately 3429 cm⁻¹ is attributed to the stretching vibration of hydroxyl (–OH) groups of PVA [59, 60]. The reduced intensity of this band compared to pure PVA is associated with the participation of hydroxyl groups in intermolecular interactions with PEO and PAAc [56, 57]. The absorption band at 1729 cm⁻¹ corresponds to the C = O stretching vibration of carboxylic acid (–COOH) groups in PAAc. The spectral region between 1000 and 1300 cm⁻¹ is mainly attributed to C–O–C stretching vibrations of PEO and PVA [58], with a characteristic peak observed at 1022 cm⁻¹ corresponding to the polymer backbone. The band at 2877 cm⁻¹ is assigned to aliphatic C–H stretching of PEO chains. Upon incorporation of TiO₂ and GO nanoparticles, specific spectral changes were observed. The band appearing near 842 cm⁻¹ is assigned to Ti–O–Ti vibrations, confirming the presence of TiO₂ within the hydrogel matrix. In contrast, the feature observed around 954 cm⁻¹ lies within the characteristic polymer vibration region and is therefore attributed to polymer backbone vibrations rather than being uniquely associated with nanoparticle incorporation. This distinction avoids overlap with polymer-related bands in the same spectral domain. Additionally, the –OH stretching band shifted to lower wavenumbers, indicating hydrogen bonding interactions between the polymer matrix and the nanoparticles. This shift is more pronounced in the GO-containing hydrogel due to the abundance of hydroxyl functional groups in GO. Similarly, the C = O stretching band at 1729 cm⁻¹ exhibited a slight shift and reduced intensity, suggesting interaction between carboxyl groups and the incorporated nanoparticles. These results confirm the successful incorporation of TiO₂ and GO and their interaction with the hydrogel network without ambiguity in peak assignment. Fig. 4FTIR spectrum of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO2a, PVA/PEO/PAAc/GOb FTIR spectrum of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO2a, PVA/PEO/PAAc/GOb XRD measurements To study the dispersion of nanoparticles within the nanocomposite hydrogel matrix, X-ray diffraction patterns were obtained. Figure 5 displays the XRD diffractogram of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO2a, and PVA/PEO/PAAc/GOb. XRD measurement of PVA/PEO/PAAc hydrogel, PVA/PEO/PAAc/TiO2a, and PVA/PEO/PAAc/GOb nanocomposite hydrogels were investigated in the 2θ ranges 4–90 °. The XRD pattern of PVA/PEO/PAAc hydrogel reveals a broad peak at around 2θ = 19 °, which represents the amorphous nature of the hydrogel, and no crystalline peak is detected [60]. However, the XRD pattern of PVA/PEO/PAAc/TiO2a shows many sharp crystalline peaks at 2θ = 23, 18, 26, and 39 °, confirming the incorporation and fine dispersion of crystalline TiO2 nanoparticles in the hydrogel matrix 66. While in the XRD pattern of PVA/PEO/PAAc/GOb, small crystalline peaks appeared at 2θ = 19 ° and 23 °, but with a smaller intensity than that observed in PVA/PEO/PAAc/TiO2. No characteristic peaks of GO were observed, as GO may have been exfoliated within the matrix [54].There is an increase in intensity of the peak at 2θ = 19.82° due to incorporation of GO content in the hydrogel matrix [60]. Fig. 5XRD pattern of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO2a, PVA/PEO/PAAc/GOb XRD pattern of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO2a, PVA/PEO/PAAc/GOb The XRD patterns reveal clear differences in crystallinity and nanoparticle dispersion among the samples. The TiO₂-containing hydrogel exhibits sharp, well-defined peaks, confirming the presence and good dispersion of crystalline TiO₂. In contrast, the GO-loaded hydrogel shows broad, low-intensity peaks, indicating a more amorphous structure. The absence of distinct GO peaks suggests that GO is highly dispersed or exfoliated within the polymer matrix. Overall, TiO₂ enhances crystallinity and structural reinforcement, while GO promotes matrix homogeneity through uniform dispersion. EDX analysis. Energy Dispersive X-ray Spectroscopy (EDX) was employed to determine the elemental composition of the prepared hydrogels. The EDX spectrum of the pristine PVA/PEO/PAAc hydrogel shows two dominant peaks corresponding to carbon (C) and oxygen (O), which are associated with the polymer backbone and the oxygen-containing functional groups of PVA, PEO, and PAAc. The absence of additional peaks confirms the purity of the hydrogel and the absence of inorganic additives [61]. For the PVA/PEO/PAAc/GO nanocomposite hydrogel, the EDX spectrum also exhibits strong C and O signals, with a noticeable increase in carbon intensity compared to the pristine hydrogel [62]. This observation is attributed to the carbon-rich structure of graphene oxide, confirming its successful incorporation into the polymer matrix. In the case of the PVA/PEO/PAAc/TiO₂ nanocomposite, additional peaks corresponding to titanium (Ti) were observed at approximately 4.5 and 4.9 keV, confirming the presence of TiO₂ nanoparticles within the hydrogel. The coexistence of C, O, and Ti peaks verifies the successful incorporation of TiO₂ into the polymer network. It should be noted that the presented results are based on EDX spectra and provide information on elemental composition only. Elemental mapping was not performed; therefore, conclusions regarding the spatial distribution or dispersion of nanoparticles are beyond the scope of this analysis. Fig. 6EDX spectra and corresponding SEM images of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂, and PVA/PEO/PAAc/GO hydrogels, showing the elemental composition and confirming the presence of C, O, and Ti elements EDX spectra and corresponding SEM images of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂, and PVA/PEO/PAAc/GO hydrogels, showing the elemental composition and confirming the presence of C, O, and Ti elements TGA analysis Thermogravimetric analysis (TGA) and derivative thermogravimetry (DTG) were used to evaluate the thermal stability and decomposition behavior of the PVA/PEO/PAAc hydrogel and its nanocomposites with TiO₂ and GO. The corresponding TGA and DTG curves are presented in Fig. 7a and b, respectively. Fig. 7a TGA and b DTG thermograms of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO2a and PVA/PEO/PAAc/GOb a TGA and b DTG thermograms of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO2a and PVA/PEO/PAAc/GOb In the TGA curves (Fig. 6a), all samples showed a gradual weight loss with increasing temperature, attributed to moisture evaporation, followed by thermal degradation of the organic polymer backbone [63]. The neat PVA/PEO/PAAc hydrogel exhibited the lowest thermal stability, with major weight loss beginning around 250 °C and completing near 500 °C. The incorporation of TiO₂ and GO significantly enhanced thermal resistance, delaying decomposition. The GO-based nanocomposite showed the most rapid weight loss beyond 300 °C, likely due to thermal degradation of oxygen-rich GO functional groups. Meanwhile, the TiO₂-containing hydrogel exhibited a more gradual decomposition profile, indicating improved structural integrity [64]. The DTG curves (Fig. 6b) further confirm the multistep degradation pattern. All hydrogels displayed three primary decomposition peaks. For PVA/PEO/PAAc, major peaks appeared at 270 °C and 340 °C, corresponding to side-chain degradation and backbone scission. In PVA/PEO/PAAc/TiO₂a, decomposition peaks shifted to 236 °C, 351 °C, and 452 °C, revealing enhanced thermal stability due to stronger interactions and crosslinking with TiO₂. Similarly, the GO-based hydrogel exhibited peaks at 270 °C and 382 °C, with a minor peak at the higher temperature, suggesting that layered GO structures delay complete degradation but initiate partial breakdown earlier. The Horowitz and Metzger method was used to determine the energy of activation (Ea), confirming the main decomposition stage of the studied samples [65, 66]. A plot of \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:\mathrm{ln}\frac{{W}_{o}-{W}_{f}}{{W}_{t}-{W}_{f}}\:\:\:$$\end{document}against θ were investigated and the slope of these curves was determined. Where, W0, Wf and Wt are the initial, final and the apparent weights of the prepared material, respectively. θ = T- Ts where T is the temperature of the sample and Ts is a reference temperature defined as the temperature where \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:\frac{{W}_{t}-{W}_{f}}{{W}_{o}-{W}_{f}}\:=1/e$$\end{document}, where R is the gas constant (R= 8.314 JK−1mol−1). The slope of the obtained straight lines equal to Ea × 1000/RTs2, where R = 8.314 J K−1 mol−1 is the gas constant. The calculated Ea values of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂ and PVA/PEO/PAAc/GO were 31.70, 32.4 and 28.92 kJ/mol, respectively. The thermal stability of PVA/PEO/PAAc was enhances after formulation with TiO₂, as reflected in the higher residual mass and delayed final decomposition. While it decreases with GO formulation. This indicates the stabilizes effects of in the polymer matrix. Adsorption of MB Effect of pH on dye adsorption The solution pH is one of the most critical parameters governing adsorption processes, as it directly affects both the ionization state of the dye molecules and the surface charge of the adsorbent [69]. Figure 7 illustrates the effect of pH on the removal percentage (R%) of methylene blue (MB) by PVA/PEO/PAAc-based hydrogels reinforced with different TiO₂ loadings (Fig. 8a) and different GO loadings (Fig.8b). For all investigated samples, MB removal efficiency increased markedly with increasing pH, reaching its maximum value at pH 10. At acidic pH values (pH 3), relatively low removal efficiencies were observed. This behavior can be attributed to the protonation of functional groups such as carboxyl (–COOH) and hydroxyl (–OH) groups on the hydrogel backbone, which leads to reduced electrostatic attraction toward the cationic MB molecules. In addition, strong hydrogen bonding under acidic conditions causes partial collapse of the hydrogel network, limiting dye diffusion into the internal adsorption sites and consequently lowering removal efficiency. As the pH increased toward neutral and alkaline conditions, deprotonation of the functional groups occurred, resulting in a more negatively charged hydrogel surface. This enhanced electrostatic attraction between the negatively charged adsorption sites and the positively charged MB molecules significantly improved dye uptake. At pH 10, near-maximum removal efficiencies were achieved for all nanocomposite hydrogels, indicating favorable adsorption conditions and effective interaction between MB molecules and the active sites of the adsorbents. Fig. 8Effect of solution pH on the removal efficiency (R%) of methylene blue (MB) by a PVA/PEO/PAAc/TiO₂ nanocomposite hydrogels with different TiO₂ loadings and b PVA/PEO/PAAc/GO nanocomposite hydrogels with different GO loadings. (Experimental conditions: initial MB concentration = 20 mg /L, adsorbent dosage = 0.10 g, solution volume = 50 mL, contact time = 24 h) Effect of solution pH on the removal efficiency (R%) of methylene blue (MB) by a PVA/PEO/PAAc/TiO₂ nanocomposite hydrogels with different TiO₂ loadings and b PVA/PEO/PAAc/GO nanocomposite hydrogels with different GO loadings. (Experimental conditions: initial MB concentration = 20 mg /L, adsorbent dosage = 0.10 g, solution volume = 50 mL, contact time = 24 h) The incorporation of TiO₂ nanoparticles (Fig. 7a) and GO nanosheets (Fig. 7b) into the PVA/PEO/PAAc hydrogel matrix led to a substantial enhancement in MB removal efficiency across the entire pH range. This improvement can be attributed to the high specific surface area of the nanofillers and the presence of abundant surface functional groups, which provide additional adsorption sites and strengthen dye–adsorbent interactions. In particular, the charged metal oxide nanoparticles promote electrostatic interactions with MB, while GO contributes π–π interactions and hydrogen bonding, further facilitating dye adsorption. Among the investigated compositions, nanocomposite hydrogels containing 1 wt% TiO₂ and 2 wt% GO exhibited the highest MB removal efficiency, especially under alkaline conditions. The overall MB removal performance followed the order: \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$ {\text{PVA/PEO/PAAc < PVA/PEO/PAAc/TiO}}_{{{\mathrm{2a}}}} {\text{ < PVA/PEO/PAAc/GO}}_{{\mathrm{b}}} $$\end{document} At higher TiO₂ or GO contents, a slight decrease in removal efficiency was observed. This behavior is likely due to the formation of a more compact hydrogel network, as excessive nanoparticle loading can act as additional physical crosslinking points [67]. Such densification reduces the available free volume and limits dye diffusion and accessibility to internal adsorption sites, thereby decreasing overall removal efficiency [68]. Effect of adsorbent weight The effect of adsorbent weight on the removal efficiency (R%) and adsorption capacity (qe) of methylene blue (MB) was evaluated over the range of 0.10 g at pH 10, initial MB concentration of 20 mg/L, solution volume of 50 mL, and contact time of 24 h, as presented in Fig. 9. The removal efficiency increased progressively with increasing adsorbent mass for all hydrogel systems. The pristine PVA/PEO/PAAc hydrogel exhibited an increase in MB removal from approximately 40% at 0.02 g to about 64% at 0.10 g. A more significant improvement was observed upon incorporation of nanofillers. Fig. 9Effect of adsorbent dosage on the removal efficiency (R%) of methylene blue (MB) by PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂, and PVA/PEO/PAAc/GO hydrogels at pH 10. Experimental conditions: initial MB concentration = 20 mg /L, solution volume = 50 mL, contact time = 24 h Effect of adsorbent dosage on the removal efficiency (R%) of methylene blue (MB) by PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂, and PVA/PEO/PAAc/GO hydrogels at pH 10. Experimental conditions: initial MB concentration = 20 mg /L, solution volume = 50 mL, contact time = 24 h The TiO₂-containing hydrogel showed removal efficiencies rising from nearly 55% to about 98%, while the GO-reinforced hydrogel achieved the highest performance, increasing from approximately 65% to nearly 100% at 0.10 g. The enhancement in removal efficiency with increasing adsorbent dosage is attributed to the greater availability of active adsorption sites and the increased surface area accessible for dye uptake, leading to more effective interaction between MB molecules and the hydrogel matrix under alkaline conditions (pH 10), where electrostatic attraction is maximized. Among the investigated systems, the adsorption performance followed the order PVA/PEO/PAAc < PVA/PEO/PAAc/TiO₂ < PVA/PEO/PAAc/GO, confirming the beneficial role of nanofiller incorporation. The superior performance of GO-containing hydrogels can be attributed to their high specific surface area and abundant oxygen-containing functional groups, which enhance electrostatic interactions and possible π–π interactions with MB molecules. Therefore, an adsorbent dosage of 0.10 g at pH 10 was identified as the optimal condition for achieving near-complete MB removal under the experimental parameters investigated. Effect of initial dye concentration and adsorption isotherm analysis Figure 10 illustrates the effect of the initial methylene blue (MB) concentration (10–50 mg L⁻¹) on the removal efficiency of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂a, and PVA/PEO/PAAc/GOb hydrogels under optimized conditions (pH = 10, adsorbent dosage = 0.10 g, contact time = 24 h). Fig. 10Effect of initial methylene blue (MB) concentration (10–50 mg L⁻¹) on removal efficiency (%) of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂a, and PVA/PEO/PAAc/GOb hydrogels. Experimental conditions: pH = 10, adsorbent dosage = 0.10 g, solution volume = 50 mL, and contact time = 24 h Effect of initial methylene blue (MB) concentration (10–50 mg L⁻¹) on removal efficiency (%) of PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂a, and PVA/PEO/PAAc/GOb hydrogels. Experimental conditions: pH = 10, adsorbent dosage = 0.10 g, solution volume = 50 mL, and contact time = 24 h The removal efficiency decreased progressively with increasing initial concentration for all investigated systems. The pristine PVA/PEO/PAAc hydrogel showed a pronounced decline from approximately 90% at 10 mg /L to about 31% at 50 mg /L, indicating rapid saturation of available adsorption sites. In contrast, the nanocomposite hydrogels exhibited significantly improved performance and greater resistance to concentration increase. The TiO₂-containing hydrogel-maintained removal efficiencies above 85% even at higher concentrations, while the GO-based hydrogel demonstrated the highest adsorption efficiency, decreasing only slightly from ~ 100% to ~ 90% across the studied range. The observed decrease in removal efficiency at elevated concentrations is attributed to progressive occupation of active adsorption sites and increased competition among MB molecules. At low concentrations, the number of active sites exceeds the number of dye molecules, enabling nearly complete removal. As concentration increases, the fixed number of adsorption sites becomes limiting, resulting in reduced percentage removal. The superior performance of GO-reinforced hydrogels can be attributed to their high surface area and abundant oxygen-containing functional groups, which enhance electrostatic attraction and π–π interactions with MB molecules. Similarly, TiO₂ incorporation improves adsorption through additional surface-active sites and stronger dye–adsorbent interactions. To further elucidate the adsorption mechanism, the equilibrium data were fitted using the Langmuir and the Freundlich isotherm models (Fig. 11a and b). The corresponding isotherm constants and statistical fitting parameters are summarized in Table 3. The Langmuir model, which assumes monolayer adsorption onto a homogeneous surface, showed excellent agreement with the experimental data, as indicated by high correlation coefficients (R² > 0.99). The calculated maximum monolayer adsorption capacities (Qₘ) confirmed that nanocomposite hydrogels possess significantly higher adsorption capacities compared to the pristine hydrogel [69]. The GO-based system exhibited high adsorption affinity (high Ka), indicating a strong interaction between MB molecules and the adsorbent surface. The Freundlich model (Fig. 11b), which describes heterogeneous multilayer adsorption, also demonstrated excellent fitting for all systems. The Freundlich constant (Kf) was highest for the GO-containing hydrogel, reflecting superior adsorption capacity. Additionally, the values of the heterogeneity parameter (n) were greater than unity for all adsorbents, confirming favorable adsorption behavior. The simultaneous good fitting to both models suggests that MB adsorption involves predominant monolayer coverage with contributions from surface heterogeneity. Figure 11c presents the dimensionless separation factor (RL), calculated from the Langmuir constant. Langmuir constant \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{K}_{a}$$\end{document}according to: \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{R}_{L}=\frac{1}{1+{K}_{a}{C}_{0}}$$\end{document}where \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{C}_{0}$$\end{document}is the initial dye concentration. The \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{R}_{L}$$\end{document}parameter provides insight into the favorability of adsorption: All (RL) values fall within the range (0 < RL< 1), confirming favorable adsorption across the studied concentration range. Moreover, (RL) decreases with increasing initial concentration, indicating enhanced adsorption favorability at higher dye concentrations. Among the investigated materials, the GO-based hydrogel consistently exhibited the lowest (RL) values, confirming its superior adsorption affinity. Fig. 11Adsorption isotherm modeling of MB removal by PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂a, and PVA/PEO/PAAc/GOb hydrogels: a Langmuir isotherm fitting, b Freundlich isotherm fitting, c Langmuir separation factor (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{R}_{L}$$\end{document}) as a function of initial dye concentration Adsorption isotherm modeling of MB removal by PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂a, and PVA/PEO/PAAc/GOb hydrogels: a Langmuir isotherm fitting, b Freundlich isotherm fitting, c Langmuir separation factor (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{R}_{L}$$\end{document}) as a function of initial dye concentration Table 3Langmuir and Freundlich isotherm parameters for MB adsorption onto PVA/PEO/PAAc-based hydrogels at pH 10 (0.10 g adsorbent, 50 mL, 24 h)SampleLangmuir Model \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{\boldsymbol{q}}_{\boldsymbol{e}}=\frac{{\boldsymbol{q}}_{\boldsymbol{m}\boldsymbol{a}\boldsymbol{x}}{\boldsymbol{K}}_{\boldsymbol{L}}{\boldsymbol{C}}_{\boldsymbol{e}}}{1+{\boldsymbol{K}}_{\boldsymbol{L}}{\boldsymbol{C}}_{\boldsymbol{e}}}$$\end{document} Freundlich Model \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{\:\boldsymbol{q}}_{\boldsymbol{e}}={{\boldsymbol{K}}_{\boldsymbol{F}}{\boldsymbol{C}}_{\boldsymbol{e}}^{1/{\boldsymbol{n}}_{\boldsymbol{f}}}}_{}$$\end{document} (Qm) (mg/g)(Ka) (L/mg)R²(Kf)(n)R²PVA/PEO/PAAc7.940.9480.999414.736.530.99963PVA/PEO/PAAc/TiO₂a27.080.4540.9932610.422.870.99851PVA/PEO/PAAc/GOb25.951.2650.9981615.214.120.99983 Table 3Langmuir and Freundlich isotherm parameters for MB adsorption onto PVA/PEO/PAAc-based hydrogels at pH 10 (0.10 g adsorbent, 50 mL, 24 h)SampleLangmuir Model \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{\boldsymbol{q}}_{\boldsymbol{e}}=\frac{{\boldsymbol{q}}_{\boldsymbol{m}\boldsymbol{a}\boldsymbol{x}}{\boldsymbol{K}}_{\boldsymbol{L}}{\boldsymbol{C}}_{\boldsymbol{e}}}{1+{\boldsymbol{K}}_{\boldsymbol{L}}{\boldsymbol{C}}_{\boldsymbol{e}}}$$\end{document} Freundlich Model \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{\:\boldsymbol{q}}_{\boldsymbol{e}}={{\boldsymbol{K}}_{\boldsymbol{F}}{\boldsymbol{C}}_{\boldsymbol{e}}^{1/{\boldsymbol{n}}_{\boldsymbol{f}}}}_{}$$\end{document} (Qm) (mg/g)(Ka) (L/mg)R²(Kf)(n)R²PVA/PEO/PAAc7.940.9480.999414.736.530.99963PVA/PEO/PAAc/TiO₂a27.080.4540.9932610.422.870.99851PVA/PEO/PAAc/GOb25.951.2650.9981615.214.120.99983 Langmuir and Freundlich isotherm parameters for MB adsorption onto PVA/PEO/PAAc-based hydrogels at pH 10 (0.10 g adsorbent, 50 mL, 24 h) Effect of contact time and kinetic study Figure 12 illustrates the effect of contact time on MB removal efficiency for PVA/PEO/PAAc and its TiO₂ and GO nanocomposite hydrogels under optimized conditions (C₀ = 20 mg /L, pH 10, 0.10 g adsorbent, 50 mL). The adsorption process proceeded rapidly during the initial 5–10 h for all samples, followed by a slower approach toward equilibrium. This rapid initial uptake is attributed to the availability of abundant active adsorption sites on the hydrogel surface. As time progressed, the adsorption rate decreased due to the gradual occupation of these sites and the reduced concentration gradient. Fig. 12Effect of contact time on MB removal efficiency by PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂a, and PVA/PEO/PAAc/GOb hydrogels under optimized conditions (C₀ = 20 mg /L, pH = 10, adsorbent dosage = 0.10 g, solution volume = 50 mL, contact time up to 30 h) Effect of contact time on MB removal efficiency by PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂a, and PVA/PEO/PAAc/GOb hydrogels under optimized conditions (C₀ = 20 mg /L, pH = 10, adsorbent dosage = 0.10 g, solution volume = 50 mL, contact time up to 30 h) The equilibrium was reached at approximately 24 h with removal efficiencies of 64% for PVA/PEO/PAAc, 98% for PVA/PEO/PAAc/TiO₂a, and nearly 100% for PVA/PEO/PAAc/GOb. The enhanced adsorption performance of the nanocomposite hydrogels is attributed to the presence of TiO₂ and GO nanoparticles, which increase surface area, introduce additional functional groups, and enhance electrostatic interactions with the cationic MB molecules. The adsorption kinetics of methylene blue (MB) onto PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂a, and PVA/PEO/PAAc/GOb hydrogels were evaluated using non-linear pseudo-first-order (PFO) and pseudo-second-order (PSO) models (Fig. 13a, b), and the resulting kinetic parameters are presented in Table 4. Although both kinetic models yielded high correlation coefficients (R² ≈ 0.999), model selection was based on the agreement between calculated and experimental equilibrium capacities. The PFO model produced \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{e,}$$\end{document}values that were closer to \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{e,\mathrm{e}\mathrm{x}\mathrm{p}}$$\end{document}for all samples, with comparatively lower deviation (Δq%) than PSO. In particular, the PVA/PEO/PAAc/GOb hydrogel showed excellent agreement with the PFO prediction (Δq% = 5.2%), while PVA/PEO/PAAc, and PVA/PEO/PAAc/TiO₂a showed moderate deviations (34.2% and 17.1%, respectively). In contrast, the PSO model substantially overestimated \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{e}$$\end{document}for all systems, resulting in higher Δq% values. Therefore, although the pseudo-second-order (PSO) model exhibited strong fitting performance (Fig. 12b), the overall kinetic behavior of MB adsorption is more consistently described by the pseudo-first-order (PFO) model based on the lower deviation (Δq%) and better agreement between calculated and experimental equilibrium capacities. This indicates that the adsorption rate is predominantly controlled by the availability of active surface sites and external mass-transfer or diffusion processes rather than being governed solely by a chemisorption-controlled mechanism [70]. The higher rate constant \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{k}_{1}$$\end{document}obtained for the GO-containing hydrogel further confirms its faster adsorption kinetics, which can be attributed to its larger surface area and stronger dye–surface interactions (electrostatic attraction and π–π interactions), resulting in both rapid uptake and higher removal efficiency [71]. The superior performance of GO-containing hydrogels reflects stronger π–π interactions and electrostatic attraction between negatively charged functional groups and the cationic MB dye [72]. Fig. 13a Pseudo-first-order kinetic model fitting for MB adsorption onto PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂a, and PVA/PEO/PAAc/GOb hydrogels. b Pseudo-second-order kinetic model fitting for MB adsorption under the same experimental conditions a Pseudo-first-order kinetic model fitting for MB adsorption onto PVA/PEO/PAAc, PVA/PEO/PAAc/TiO₂a, and PVA/PEO/PAAc/GOb hydrogels. b Pseudo-second-order kinetic model fitting for MB adsorption under the same experimental conditions Table 4Kinetic parameters obtained from pseudo-first-order and pseudo-second-order models for MB adsorption onto PVA/PEO/PAAc-based hydrogelsSamplePFO: \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{t}={q}_{e}\left(1-{e}^{-{k}_{1}t}\right)$$\end{document}PSO: \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{t}=\frac{{k}_{2}{q}_{e}^{2}t}{1+{k}_{2}{q}_{e}t}$$\end{document} \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{e,\:exp\:}$$\end{document} \:(mg/g) \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{e,\:cal}$$\end{document} \:(mg/g) \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{k}_{1},$$\end{document} \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:\left({h}^{-1}\right)$$\end{document} R² \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:\varDelta\:q\left(\%\right)$$\end{document} \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{e,\:cal}$$\end{document} \:(mg/g) \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{k}_{2},$$\end{document} \:(g mg⁻¹ h⁻¹\:)R² \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:\varDelta\:q\left(\%\right)$$\end{document} PVA/PEO/PAAc6.408.590.05160.999634.2213.590.002480.9995112.34PVA/PEO/PAAc/TiO₂a9.8011.480.07200.999417.1416.640.003240.999369.80PVA/PEO/PAAc/GOb10.0010.520.11000.99895.2013.950.006880.999839.50 Table 4Kinetic parameters obtained from pseudo-first-order and pseudo-second-order models for MB adsorption onto PVA/PEO/PAAc-based hydrogelsSamplePFO: \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{t}={q}_{e}\left(1-{e}^{-{k}_{1}t}\right)$$\end{document}PSO: \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{t}=\frac{{k}_{2}{q}_{e}^{2}t}{1+{k}_{2}{q}_{e}t}$$\end{document} \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{e,\:exp\:}$$\end{document} \:(mg/g) \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{e,\:cal}$$\end{document} \:(mg/g) \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{k}_{1},$$\end{document} \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:\left({h}^{-1}\right)$$\end{document} R² \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:\varDelta\:q\left(\%\right)$$\end{document} \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{e,\:cal}$$\end{document} \:(mg/g) \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{k}_{2},$$\end{document} \:(g mg⁻¹ h⁻¹\:)R² \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:\varDelta\:q\left(\%\right)$$\end{document} PVA/PEO/PAAc6.408.590.05160.999634.2213.590.002480.9995112.34PVA/PEO/PAAc/TiO₂a9.8011.480.07200.999417.1416.640.003240.999369.80PVA/PEO/PAAc/GOb10.0010.520.11000.99895.2013.950.006880.999839.50 Kinetic parameters obtained from pseudo-first-order and pseudo-second-order models for MB adsorption onto PVA/PEO/PAAc-based hydrogels The isotherm and kinetic analyses indicate that MB adsorption onto the prepared PVA/PEO/PAAc-based hydrogels is best described by the Langmuir isotherm and the pseudo-first-order kinetic model. The strong conformity with the Langmuir model suggests that adsorption occurs predominantly as monolayer coverage on relatively homogeneous active sites. In addition, the close agreement between calculated and experimental \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{q}_{e}$$\end{document}values, together with low deviation percentages, confirms the suitability of the PFO model in representing the adsorption kinetics. The kinetic behavior further implies that the rate-controlling step is governed mainly by surface-site availability and diffusion processes. Overall, the adsorption mechanism is primarily physical in nature, driven by electrostatic interactions and van der Waals forces between MB molecules and the functional groups of the hydrogel matrix. Table 5 presents a comparison of the adsorption capacity (qe, mg/g) of the prepared hydrogels with various reported adsorbents for methylene blue (MB) removal under different experimental conditions. It should be noted that direct comparison between materials may be influenced by differences in operating parameters such as initial dye concentration and pH. Nevertheless, the PVA/PEO/PAAc/GO nanocomposite exhibited competitive adsorption performance, achieving a qe value of 10 mg/g under the conditions of pH 10, initial concentration of 20 mg/L, adsorbent dosage of 0.10 g, and contact time of 24 h. Table 5The adsorption of MB onto different sorbentMaterialConcentration (mg/L)qe (mg/g)pHReferencesCMGG/PAAc40493 [73]CMC-Alg/GO1516.639.5 [74]Alginate/polyaspartate104.85 [75]PVA-5.26.3 [76]PEO-38.36.3 [76]CMC coated Fe3O4@SiO2 nanocomposite7022.711 [77]PVA/D- glucose/agar-29- [78]PVA/PEO/PAAc206.410This workPVA/PEO/PAAc/TiO2a209.810PVA/PEO/PAAc/GOb201010 Table 5The adsorption of MB onto different sorbentMaterialConcentration (mg/L)qe (mg/g)pHReferencesCMGG/PAAc40493 [73]CMC-Alg/GO1516.639.5 [74]Alginate/polyaspartate104.85 [75]PVA-5.26.3 [76]PEO-38.36.3 [76]CMC coated Fe3O4@SiO2 nanocomposite7022.711 [77]PVA/D- glucose/agar-29- [78]PVA/PEO/PAAc206.410This workPVA/PEO/PAAc/TiO2a209.810PVA/PEO/PAAc/GOb201010 The adsorption of MB onto different sorbent Conclusion In this study, PVA/PEO/PAAc-based nanocomposite hydrogels incorporating TiO₂ and graphene oxide (GO) were successfully synthesized via gamma irradiation–induced copolymerization at a total dose of 30 kGy. The incorporation of nanofillers improved the physicochemical properties of the hydrogel network, including gel fraction and swelling behavior, with the highest swelling observed under alkaline conditions (pH 10) after 24 h. Comprehensive characterization (FTIR, TGA, AFM, XRD, SEM, and EDX) confirmed the successful incorporation of TiO₂ and GO within the polymer matrix and revealed distinct structural roles for each filler. GO contributed to increased surface roughness, porosity, and availability of functional groups, whereas TiO₂ enhanced crystallinity and thermal stability of the hydrogel system. The adsorption performance toward methylene blue (MB) dye demonstrated a clear improvement upon nanofiller incorporation, following the trend: PVA/PEO/PAAc < PVA/PEO/PAAc/TiO₂ < PVA/PEO/PAAc/GO. Under the investigated conditions (pH 10, 24 h, 20 mg/L MB), the maximum removal efficiencies reached 64%, 98%, and ~ 100%, respectively. Isotherm analysis showed better agreement with the Langmuir model, suggesting predominantly monolayer adsorption behavior, while kinetic data were more consistent with a pseudo-first-order model, indicating that physisorption plays a major role in the adsorption process. Overall, GO was more effective in enhancing adsorption performance due to its high surface area and abundant oxygen-containing functional groups, whereas TiO₂ primarily contributed to improved structural integrity and thermal resistance. These results highlight that the selection of nanofiller can be tuned depending on whether adsorption efficiency or material stability is the primary target. Limitations and future perspectives Despite these promising results, several limitations should be acknowledged. The adsorption experiments were conducted under controlled batch conditions using a single model dye (methylene blue), which may not fully represent the complexity of real wastewater systems containing mixed pollutants. Future work should therefore focus on evaluating the performance of these hydrogels in real wastewater matrices, assessing their recyclability and long-term stability, and employing advanced characterization and modeling approaches to better understand the adsorption mechanisms and optimize material design for scalable applications. Supporting information summary Our experimental procedures, including the materials used, the experimental steps for preparation of hydrogel nanocomposites, in addition to characterization techniques by different instruments, FTIR, XRD, and AFM, are presented with the supporting information in our current manuscript by providing figures and tables.