Microsphere‐Templated Conductive Syntactic Foams for Recyclable and Additively Manufactured Soft Electronics Authors: Gayaneh Petrossian, Yassine Diouri, Bolan Xu, Sara Ebrahimi, Atharva Pande, Floriane Miquet‐Westphal, Hang Xu, Fabio Cicoira Published: 2026 ABSTRACT ABSTRACTSoft, conductive materials that simultaneously offer mechanical compliance, electrical conductivity, recyclability, and scalable manufacturing remain difficult to achieve. Here, we introduce recyclable, 3D‐printable PEDOT:PSS syntactic foams based on polymer microspheres coated in situ, enabling precise control over porosity, mechanical properties, and electrical conductivity. Microsphere‐templated conductive shells provide a unique materials architecture that unites porosity control, tailorable flexibility, electrical functionality, recyclability, and additive manufacturability, which are capabilities that are challenging to achieve in conventional conductive foams. The resulting foams exhibit low elastic moduli comparable to soft biological tissues, stable electrical conductivity over a wide void‐fraction range, and excellent compatibility with fused filament fabrication. Importantly, the foams can be thermally reshaped, and the conductive microsphere component can be recovered from the matrix by selective dissolution, while preserving structural integrity and electrical performance. To demonstrate functional relevance, the conductive foams are integrated into soft wearable electrodes, enabling reliable acquisition of electrocardiogram (ECG), electromyogram (EMG), and in‐ear electroencephalogram (EEG) signals, including clear alpha‐band modulation. Overall, this work establishes conductive syntactic foams as a recyclable and manufacturable materials platform for soft and wearable electronic systems. Introduction The increasing demand for materials that are versatile yet lightweight has driven the advancement of multifunctional cellular foams. Due to their tailorable constituents and porous‐structure‐induced low density, these foams offer a unique combination of properties such as shock absorption, thermal insulation, vibration damping, and cushioning, making them indispensable across various industrial sectors, ranging from packaging to construction [1]. More recently, attention has shifted toward functional foams that go beyond conventional applications, for example, by incorporating electrical conductivity to expand their potential uses in wearable bioelectronics [2, 3, 4, 5] and energy storage [6, 7, 8]. This multifunctionality positions conductive foams as a new generation of materials capable of addressing both structural and electronic demands in wearable devices, such as an ear‐electroencephalograph (ear‐EEG), which requires soft, low‐density, and conformal electrodes that can maintain good electrical contact in the confined and curved ear canal geometry [9, 10]. Conductive foams generally integrate conductive fillers, such as carbon nanotubes [11], graphene [12], and metallic powders [13] in polymer matrices via various foaming techniques to achieve tailored electrical and mechanical properties. Producing conductive foams is inherently challenging due to the need for uniformly dispersed fillers that ensure a continuous conductive network (percolation) without compromising the foam's lightweight structure and desired porosity. Additionally, strong adhesion between the fillers and the polymer matrix is critical for maintaining durability and consistent performance under mechanical stress or environmental exposure [14, 15]. However, the presence of conductive fillers alters viscosity and destabilizes bubbles, thereby interfering with the foaming process and complicating the balance between conductivity and structural integrity. Material compatibility and scalability also pose hurdles, requiring precise control over processing parameters to achieve uniformity and stability in large‐scale production. These challenges necessitate innovative approaches to optimize the fabrication and functionality of conductive foams. Recently, 3D‐printable foams have gained significant attention because they offer design freedom, rapid prototyping, and the ability to tailor lightweight cellular structures [16]. The main strategies include syntactic foams [17], post‐foaming of printed solids [18, 19], and in situ foaming of gas‐ or blowing‐agent–saturated filaments [20, 21]. Recycling is a critical consideration for sustainable foam production, yet conventional foams generally lose their cellular architecture when melted or dissolved, requiring energy‐intensive re‐foaming to restore functionality. When conventional foamed polymers are 3D‐printed through extrusion and layered sequentially, such as via the fused filament fabrication (FFF) method, their fragile porous architecture often collapses or degrades. Gas bubbles can merge into larger voids or dissipate under heat and shear forces, leading to structural instability and inconsistency in the printed component. Therefore, controlling pore distribution and retention during FFF remains a significant challenge. Syntactic foams, which incorporate hollow microspheres (comprising glass, polymer, or ceramic) into a matrix, offer a promising alternative. Initially used in marine structures by virtue of their buoyancy [22], hollow microspheres have recently gained attention for their ease of processing, scalability, and superior mechanical properties [23, 24, 25]. The pre‐engineered, thermally stable microspheres maintain their integrity during reprocessing, so the bulk matrix can be melted and reshaped without destroying the porous structure. When the ease of processing and the rapid prototyping advantages of additive manufacturing are combined with the inherent recyclability of syntactic foams, it results in a highly versatile platform that enables efficient reuse, reshaping, and even self‐healing while preserving both mechanical and additional functional performance. Building on these advantages, researchers have explored strategies to functionalize syntactic foams by coating microspheres with conductive or protective layers to improve interfacial properties and multifunctionality [26, 27, 28, 29, 30, 31]. For example, polydopamine (PDA) has been employed as a versatile surface treatment layer on hollow carbon microspheres to enhance interfacial adhesion with polymer matrices. In addition to improving mechanical integration, PDA can serve as an effective anchoring platform for secondary metallic coatings, such as silver, enabling the fabrication of lightweight foams with high electromagnetic interference (EMI) shielding effectiveness [30]. Similarly, silver‐coated hollow glass microspheres fabricated via in situ composite technique in the presence of polyvinylpyrrolidone (PVP), have achieved tunable shell thickness and shielding effectiveness values up to 70–80 dB in the GHz range [28]. More recently, multifunctional syntactic foams have been reported using silver‐ and nickel‐plated microspheres embedded in shape‐memory vitrimer matrices, enabling multi‐functionality of conductivity, ferromagnetism, and recyclability [29]. While these studies demonstrate the promise of conductive syntactic foams, they are often constrained by high costs due to the use of metals, overall heavier weight compared to conventional foams due to the presence of metals that increase density, and possible long‐term instability arising from metal oxidation. Alternative conductive materials for coating hollow microspheres require further investigation. To overcome these limitations, some researchers have begun incorporating Poly(3,4‐ethylenedioxythiophene)‐poly(styrenesulfonate) (PEDOT:PSS) into porous foam structures, which offer a promising route to combine electrical functionality with the mechanical benefits of lightweight, flexible, and conformable architectures. PEDOT:PSS is a widely studied conductive polymer known for its conductivity, biocompatibility, and ease of processing. It has been extensively used in thin‐film and hydrogel systems for electronic and bioelectronic applications. However, extending PEDOT:PSS to 3D porous architectures remains challenging due to its inherent brittleness in the solid state and its water‐based, hygroscopic nature, which limits compatibility and homogeneous mixing with many thermoplastic matrices. These limitations make it difficult to form stable micro‐porous conductive foams with well‐defined and continuous conductive pathways. These challenges are further exacerbated in additive manufacturing processes such as fused filament fabrication (FFF), where maintaining both pore structure and conductive network integrity under thermal and shear stresses is particularly difficult. Overcoming these challenges is particularly critical for developing 3D, multifunctional sensing platforms that require materials that are conductive, biocompatible, and also mechanically robust and adaptable. Recent research has therefore focused on using alternative processing methods, such as blending‐molding [32] and electrodeposition [33], to adapt PEDOT:PSS into architectures with varied geometries and functionalities. Various fabrication methods, such as freeze‐drying [34, 35], dip‐coating [36, 37, 38], and addition of foaming agents [3, 39] have been employed to create PEDOT:PSS‐based foams. However, these approaches remain difficult to translate to fused filament fabrication, where achieving uniform dispersion of the conductive phase while preserving pore structure under thermal and shear stresses is particularly challenging. While these studies demonstrate the materials’ potential in wearable and flexible sensors, opportunities remain to further control pore size and distribution, which are key to optimizing both mechanical strength and electrical performance. To address these challenges, we adopt a microsphere‐templated strategy in which PEDOT:PSS is synthesized directly on the surface of hollow polymer microspheres, localizing conductivity at the microsphere interface while preserving the porous architecture and enabling compatibility with additive manufacturing processes, such as FFF. Here, we demonstrate conductive polymer foams that are simultaneously 3D‐printable and thermally reprocessable, while retaining mechanical and electrical performance over multiple reprocessing cycles. By incorporating PEDOT:PSS‐coated polymer microspheres into a thermoplastic poly(ε‐caprolactone) matrix, we establish a scalable and straightforward materials strategy for fabricating lightweight syntactic foams with tunable porosity, electrical conductivity, and mechanical robustness suited to flexible bioelectronics. Localizing electrical functionality at the microsphere surface simplifies the fabrication of conductive foams compared to conventional approaches that rely on complex formulations incorporating carbon‐based or metallic fillers. Importantly, the foams preserve their functionality through dual recyclability, either by selective matrix dissolution to recover intact conductive microspheres or by thermal reshaping into new geometries without performance loss. Collectively, these capabilities demonstrate that the proposed microsphere‐templated conductive foam represents a versatile materials platform that simultaneously enables additive manufacturing, recyclability, and bioelectronic functionality. Results and Discussion PEDOT:PSS‐Covered Microsphere Preparation An in situ oxidative polymerization strategy was employed to prepare PEDOT:PSS‐coated microspheres, as schematically illustrated in Figure 1a. The visual evolution of the powders with different synthesis durations of 2, 4, 8, 12, and 24 h, shown in Figure 1b, clearly reflects the progression of polymerization: the color gradually shifts from white to dark blue as the reaction time increases, indicative of PEDOT:PSS formation and increasing coating thickness. (a) Schematic of the preparation process of the conductive microsphere. (b) Digital images showing the color evolution of the powders from off‐white (as‐received bare microspheres) to dark blue with increasing polymerization time (2–24 h), indicating progressive formation and thickening of the PEDOT:PSS coating. Schematic created with BioRender. (c) SEM images of (c1) bare microspheres (MS), (c2‐c3) MS after 12, and 24 h of in situ PEDOT:PSS polymerization, (c4) MS coated with PEDOT:PSS PH1000. Figure 1c presents SEM images of pristine microspheres (MS) and those subjected to in situ PEDOT:PSS polymerization for various reaction durations, along with MS coated with commercial PEDOT:PSS. The pristine MS (Figure 1c1 ) exhibited smooth surface morphologies with occasional shallow dimples, characteristic of the Expancel shell. With increased reaction time (Figure 1c2 ), a thin PEDOT:PSS layer progressively formed on the surface, initially imparting only subtle texture changes. Dark, irregular patches were observed, indicating thicker PEDOT:PSS deposits. The small, round spots visible on the surface in Figure 1c2 likely result from microspheres adhering to each other during drying and later being separated by sieving, which causes PEDOT:PSS‐coated regions to detach from one microsphere and reattach to another. After 24 h (Figure 1c3 ), the microspheres exhibited a significantly roughened and continuous coating layer, suggesting near‐complete surface coverage and the formation of a conductive shell, which correlates with the onset of electrical conductivity observed for the corresponding samples. In contrast, the sample prepared by mixing MS with PEDOT:PSS PH1000 followed by drying (Figure 1c4 ) displayed non‐uniform PEDOT:PSS aggregates and large flakes loosely adhered to the surface. This comparison highlights the superior uniformity, coverage, and adhesion achieved via in situ polymerization relative to the mixing method. FTIR analysis (Figure 2a) successfully tracked the in situ polymerization and deposition of PEDOT:PSS onto the MS over time. The bare MS spectrum established the baseline for the pristine polymer shell. As the synthesis time increased from 2 h to 24 h, the spectra clearly transitioned from being dominated by the native MS peaks to showing strong, characteristic signals of the conductive polymer. This confirms the formation of a continuous and thickening PEDOT:PSS layer on the MS surface. (a) FTIR spectra of bare MS, PEDOT:PSS film, and MS after 2, 8, and 12 h of synthesis. Effect of synthesis time on microsphere properties. (b) Shell density of microspheres as a function of synthesis duration, showing a gradual increase with longer polymerization times. Error bars represent the standard deviation of three independent measurements. (c) Particle size distributions of powders obtained after 2, 8, and 24 h of synthesis. Powder percentage represents the relative volume fraction of particles within each size range as measured by laser scattering. This growth is spectroscopically confirmed by the progressive emergence and intensification of characteristic PEDOT:PSS vibrational bands, as validated through direct comparison with a reference PEDOT:PSS film synthesized separately under identical polymerization conditions [40, 41, 42]. Specifically, we observed a direct correlation between reaction time and the intensity of the C─C and C═C stretching vibrations of the PEDOT thiophene ring (∼1350–1550 cm−1, specifically at 1514 cm−1), the asymmetric/symmetric S═O stretching vibrations of the PSS dopant (∼1100–1200 cm−1, specifically at 1190 cm−1), and the C─O─C (∼970 cm−1) and C─S─C (∼830 cm−1) deformation vibrations of the PEDOT backbone. Additionally, the S─O bending vibrations of the PSS sulfonate group (∼690 cm−1) grew stronger. This comprehensive spectral evolution directly supports the morphological finding that extended synthesis time yields more pronounced surface coverage and thicker PEDOT:PSS deposits. To further confirm PEDOT:PSS deposition and quantify its contribution to the total mass of the MS shell (e.g., the polymer wall of the hollow microspheres), a helium pycnometer was used to measure the effective shell density before and after coating (Figure 2b). Because helium can permeate through the polymer shell and surface defects, the internal void volume is excluded from the measured volume, and the measurement reflects only the density of the solid shell material. The pristine MS exhibited a shell density of 1.12 ± 0.02 g cm−3, which, with polymerization time, gradually increased to 1.48 ± 0.08 (8 h), 2.15 ± 0.07 (12 h), and 2.23 ± 0.15 g cm−3 (24 h), reflecting progressive PEDOT:PSS deposition and correlating with SEM observations of thicker coatings. Although the overall density of the hollow microspheres is still largely governed by the internal void, the rise in shell density contributes to an increase in the total particle density once the coating is sufficiently thick. The effect of polymerization time on particle size distribution, and consequently on the final microsphere size, was further evaluated by a laser scattering analyzer (Figure 2c). In this plot, the y‐axis represents the relative proportion of particles within each size range, providing a measure of the particle size distribution for powders synthesized under different reaction times. After 2 h of reaction, the size distribution exhibited a sharp peak centered at ∼45 µm, indicating minimal growth of the PEDOT:PSS layer. Extending polymerization to 8 h led to minor broadening of the distribution and a slight shift toward larger diameters, consistent with thicker and less uniform coverage. After 24 h, this effect became more pronounced, with a broader tail extending to higher diameters, reflecting the continued surface deposition. Overall, despite continued PEDOT:PSS deposition, the overall microsphere size remains largely unchanged, reflecting the thin nature of the coating relative to the microsphere diameter. These findings are consistent with the pycnometer and SEM data, which confirm increased coating mass and thickness without major changes in particle size. Morphology of Foams Building upon the powder‐level characterization, which confirmed successful PEDOT:PSS coating and controlled particle morphology, the next stage focused on understanding how these modified microspheres influence the structure of the resulting foams. DSC thermograms of PCL and PCL‐PEDOT:PSS foams, showing a melting transition near 60°C (Figure S1a). This transition was used to define the temperature limit for thermal processing, ensuring sufficient polymer softening to enable foam shaping and consolidation. The morphology of foams with different void fractions was examined by SEM (Figure 3). Studying morphology at varying void fractions is essential, since wall thickness and microsphere packing directly influence the foam's density, mechanical compliance, and the ability to form continuous conductive pathways. At 70% void fraction (Figure 3a), the structure is composed of densely packed microspheres with relatively thick matrix walls that separate adjacent pores. This arrangement preserves mechanical stability while still reducing the bulk density by introducing a considerable amount of void space. In contrast, at 85% void fraction (Figure 3b), the foam displays a highly porous structure in which thin matrix walls surround the pores. The increased void content leads to extensive interconnection between neighboring microspheres, with the microspheres dominating the architecture as the solid matrix phase becomes progressively thinner. Cross‐sectional SEM images of PEDOT:PSS‐coated microsphere foams with (a) 70% and (b) 85% void fraction, showing the transition from thicker matrix walls to a highly porous structure with thin interconnecting walls. Enlarged views highlight increased microsphere packing at higher void fraction. Red dashed outlines mark regions of reduced matrix thickness between adjacent microspheres. Thermogravimetric analysis (TGA) was carried out to evaluate the thermal stability of CMS and the foams (Figure S1b,c). Since the coated microspheres can also be incorporated into other polymer matrices, it was important to assess their intrinsic thermal stability separately from that of the PCL‐based foams. PEDOT:PSS‐covered microspheres (Figure S1b) exhibited continuous weight loss across the entire temperature range, leaving a presumably carbonaceous solid residue yield of approximately 29% at 800°C, consistent with previous reports [43]. Since foams with an 85% void fraction were used for all subsequent tests, this composition, chosen as a representative balance between high porosity, mechanical integrity, and electrical performance, was also selected for TGA analysis to ensure consistency. For the 85% void fraction foams (Figure S1c), both uncoated and coated samples showed a major degradation step between 400–450°C, characteristic of PCL decomposition. However, the foam containing PEDOT:PSS retained a higher solid yield (19%) compared to the neat PCL foam (8%). This difference reflects the contribution of both the PEDOT:PSS coating and the Expancel microspheres, which both contribute to the formation of thermally stable residues during decomposition. Figure 4a displays a representative sample of the 85% void fraction foam, illustrating its uniformity and mechanical stability even at high porosity, while Figure 4b visually demonstrates the ultralight nature of the foam by balancing it atop a delicate flower. Density measurements (Figure 4c) provide additional insight into the role of the coated microspheres. The initial theoretical density of the foams was estimated using the density of uncoated Expancel microspheres (30 kg m−3). After foam fabrication, the density of each sample was measured and used to back‐calculate the effective volume fraction and average density of the CMS. This analysis yielded an effective conductive microsphere density of ∼66 kg m−3, more than double that of uncoated Expancel, consistent with the added PEDOT:PSS. Using this corrected CMS density, new adjusted theoretical foam densities were calculated, which showed very good agreement with experimental values, shown in Figure 4c. This confirms both the successful incorporation of PEDOT:PSS onto the microsphere surfaces and the accuracy of the foaming process in producing controlled structures across varying void fractions. Digital images of (a) the 85% foam and (b) 85% foam on a flower. (c) Comparison of theoretical, adjusted theoretical, and measured foam densities (n = 3) at different void fractions (70%, 75%, 80%, 85%). Actual density values are averaged from the density values of 3 cubic samples. (d) Electrical conductivity of foams as a function of void fraction, compared with a control prepared by simply mixing PH1000 with uncoated microspheres (mean of 3 measurements). Conductive foams reported in the literature (Table 1) span a broad density range, from ultralight graphene or PEDOT:PSS aerogel‐like systems (∼0.02–0.03 g cm−3) [44] to more conventional polymeric foams (up to ∼0.48 g cm−3) [45]. Our foams, with densities around ∼0.2 g cm−3, occupy an intermediate region that balances lightweight porosity with mechanical compliance and scalable processing. This places them in a favorable position for applications requiring both structural functionality and electrical performance, not as fragile as ultralight aerogels, yet significantly lighter than typical solid foams. TABLE 1Summary of conductive foams showing foaming method, average conductivity, and density.MaterialsFoaming MethodConductivity [S cm−1]Density [g cm−3]Ref.PCL/PEDOT:PSSSyntactic foams10−2‐10−3 0.2This workTPU/0.06vol%CNTFreeze‐drying10−3 0.123Huang et al. [46]TPU/rGOFreeze‐drying/dip‐coating0.070.162Lu et al. [47]TPU/PDA/3.45wt.%MXeneFreeze‐drying/dip‐coating2.5×10−3 0.106Chen et al. [48]MXene/auxetic PUDip‐coating/triaxial compression0.1060.063Kim et al. [49]Melamine/PEDOT:PSSDip‐coating0.580.12Gu et al. [50]TPU/CNT3D printing10−8‐10−5 0.25‐1Aghvami‐Panah et al. [51]John Wiley & Sons, Ltd. Summary of conductive foams showing foaming method, average conductivity, and density. Electrical conductivity measurements (Figure 4d) further highlight the advantage of PEDOT:PSS in situ polymerization. The control sample, prepared by mixing pristine microspheres with PH1000, exhibited low conductivity (∼10−6 S cm−1), reflecting the absence of a continuous conductive network due to poor filler dispersion and weak interfacial contact. In contrast, foams fabricated with synthesized in situ PEDOT:PSS‐coated microspheres showed conductivities several orders of magnitude higher, systematically increasing from ∼10−4 S cm−1 at 70% void fraction to ∼10−2 S cm−1 at 85%. This trend reflects the formation of percolating conductive pathways along the PEDOT:PSS coatings. At lower void fractions, conductive contacts are sparse, while at higher void fractions, increased microsphere packing enhances connectivity and facilitates efficient charge transport. In this system, a higher void fraction corresponds to a larger volume fraction of conductive microspheres, since the same component provides both porosity and conductivity. Consequently, increasing the void fraction not only increases porosity but also enriches the density of the conductive component, thereby improving electrical connectivity. Compared with other polymer foams reported in the literature (Table 1), our PEDOT:PSS‐PCL syntactic foams achieve conductivities on the order of 10−2–10−3 S cm−1, which are among the highest for polymer‐based conductive foams without metallic or carbon‐based fillers. PEDOT:PSS‐based conductive foams have been realized using a range of fabrication strategies, each associated with distinct advantages and limitations. Freeze‐drying approaches can produce highly porous structures and, in some cases, relatively moderate conductivities (e.g., 2.85 S cm−1 reported by Yun et al. [34]), but often result in foams with limited mechanical integrity due to the intrinsic brittleness of the PEDOT:PSS network. Methods based on foaming agents offer simpler processing but provide limited control over pore size and distribution, which can impact electrical performance [3, 39]. Dip‐coating strategies can achieve higher conductivity (e.g., up to ∼50 S cm−1 as reported by Thongkham et al. [38]), but rely on surface deposition of PEDOT:PSS, which may lead to adhesion issues under mechanical deformation. In contrast, the present microsphere‐templated approach enables localized conductivity within a mechanically robust and structurally stable foam, while maintaining processability and compatibility with scalable fabrication methods. Mechanical Properties Figure 5a shows the compressive behavior of the foams to assess the influence of void fraction and PEDOT:PSS incorporation on mechanical performance (refer to the Experimental Section/Methods for more information on mechanical characterization). PCL+PEDOT:PSS foams exhibit the characteristic three‐region stress‐strain response of cellular solids: an initial elastic region, a plateau region, and a final densification region [52]. Foams with lower void fractions (e.g., 70%) show higher stiffness and compressive resistance, whereas those with higher void fractions (e.g., 85%) display lower stress‐strain slopes, reflecting reduced load‐bearing capacity due to the smaller matrix content. Mechanical properties of foams. (a) Compressive stress‐strain curves of PCL+PEDOT:PSS foams with different void fractions. (b) Comparison of compressive stress–strain curves of PCL, PCL foam, and PCL+PEDOT:PSS foam at 85% void fraction. (c) Comparison of compressive modulus (error bars represent standard deviation from 4 measurements). (d) Resistance change (ΔR/R0) vs. compressive strain of 85% PCL+PEDOT:PSS foam. Data are reported as mean ± standard deviation of 4 measurements (the shaded area around the curve represents the standard deviation). In the elastic regime (0%–10% strain), lower porosity foams exhibited steeper stress slopes, reflecting a higher initial modulus. With increased porosity, the modulus decreased, and the plateau region became more pronounced, consistent with progressive buckling of the thin inter‐void walls of PCL. At higher strains (∼40%–50%), the foams transitioned into the densification region, where collapsed pores were compacted, and the material stiffened rapidly. This region appeared earlier and was more pronounced in lower porosity foams (70% and 75%) due to their greater solid content, while higher void fraction foams (80% and 85%) exhibited delayed densification, consistent with their higher porosity and enhanced capacity for deformation. As shown in Figure 5b, compared to the dense, non‐porous PCL sample, which showed a linear and brittle stress‐strain profile without a plateau, all foams demonstrated significantly greater deformability. The incorporation of PEDOT:PSS‐coated microspheres altered the mechanical response, particularly at high porosity. For instance, the elastic modulus of the 85% void fraction foam increased relative to its uncoated counterpart (Figure 5b), suggesting a higher shell rigidity. This trend was confirmed by compressive modulus values (Figure 5c), where PEDOT:PSS‐containing foams consistently showed higher modulus compared to the uncoated foams across all porosities. These results highlight the dual role of PEDOT:PSS as both a conductive and mechanically reinforcing component. Under compressive loading, the conductive foam exhibits a pronounced piezoresistive response, as shown in Figure 5d. A rapid reduction in resistance occurs at low compressive strain, followed by a more gradual and stable decrease at higher strains, reaching ΔR/R0 ≈ ‐90%, which is characteristic of porous conducting polymer foams [53, 54]. This behavior can be attributed to compression‐induced densification of the foam and increased interparticle contacts within the conductive microsphere network, which facilitate charge transport. The reproducible response highlights the suitability of the foam for compression or strain‐based electromechanical sensing. Importantly, the Young's modulus of the developed PEDOT:PSS foams falls well within the range accepted for skin‐contact applications. Recent literature reports that the effective Young's modulus of hydrated human skin spans broadly from 10 kPa to 1 MPa, depending on anatomical site and hydration state [55, 56]. By matching their moduli to this spectrum, these foams minimize mechanical mismatch at the skin–electrode interface, thereby improving comfort, conformability, and reducing motion artifacts during the collection of physiological signals. The compressive moduli observed for all foam variants in this study are accordingly well‐suited for epidermal electronics and wearable biosensor platforms, as they support both stable device contact and imperceptible integration with the user's skin. Additive Manufacturing To further demonstrate the versatility of the developed material platform, we evaluate its compatibility with fused filament fabrication (FFF), showing that the same microsphere‐templated conductive foam can support both bioelectronic function and additive manufacturing of complex geometries. The additive manufacturing process yielded PCL and PCL+PEDOT:PSS syntactic foams with consistent microstructure and excellent compatibility for commercialized 3D printers (refer to the Experimental Section/Methods for more information on additive manufacturing). For 3D printing, a lower void fraction (75%) was selected to improve processability during filament extrusion and printing. At higher void fractions, increased compressibility leads to deformation and instability during filament feeding and deposition. The 75% composition provides sufficient mechanical integrity for consistent printing while preserving the key structural and electrical characteristics of the microsphere‐templated architecture, illustrating the trade‐off between mechanical processability and functional performance. The SEM micrograph (Figure 6a) highlights the integrity of PEDOT:PSS‐coated microspheres, while printed dogbone specimens (Figure 6b) display smooth surfaces and dimensional uniformity, underscoring reliable process control. Tensile testing was used here primarily to assess fabrication repeatability, consistency, and the influence of printing direction on the mechanical response of the printed samples. Specimens were fabricated in both horizontal and vertical orientations relative to the build direction. The tensile stress‐strain curves (Figure 6c) feature shaded regions denoting standard deviation, which remains around 5% across measurements, providing quantitative evidence of reproducible fabrication and uniform mechanical properties, particularly for horizontally printed samples, which exhibit consistent behavior. The curves show an initial elastic regime followed by a stable plastic plateau, consistent with the tensile deformation behavior of polymer foams. Fabrication, morphology, and mechanical characterization of 3D‐printed 75% void fraction foams. (a) Extrusion of conductive foam filament prior to printing. The corresponding SEM image shows the cross‐section of a representative 75% PCL+PEDOT:PSS foam filament, with enlarged views showing the internal porous structure. (b) Photographs of 3D‐printed tensile dogbone specimens fabricated from neat PCL foam (top) and PCL + PEDOT:PSS foam (bottom). The corresponding SEM image shows the cross‐sectional morphology of the printed conductive foam sample. (c) Representative tensile stress‐strain curves of 75% PCL (horizontal build direction) and 75% PCL‐PEDOT:PSS foams printed in horizontal and vertical orientations (shaded regions represent standard deviation. Data are reported as mean ± standard deviation of 4 measurements). (d) As‐printed dogbone specimen in the vertical direction with supporting structures. Mechanical benchmarking reveals that adding PEDOT:PSS‐coated microspheres increases tensile modulus and yield strength but lowers strain‐at‐break compared to pure PCL foam. This is typical for conductive composite foams, since rigid filler particles introduce local stress concentrations and constrain matrix mobility, causing earlier microcrack formation and reduced elongation [57]. While this leads to lower ductility, the resulting strain‐at‐break still meets the requirements for wearable and skin‐interfaced sensors, maintaining a balance between flexibility and robustness for soft bioelectronic applications. Different stiffnesses can be achieved by altering the void fractions, highlighting the material's designability. A clear dependence on printing direction is also observed. Specimens printed in the vertical orientation exhibit reduced tensile strength compared to horizontally printed counterparts, consistent with weaker interlayer adhesion commonly observed in extrusion‐based additive manufacturing. This anisotropic behavior highlights the importance of print orientation in determining mechanical performance, particularly for load‐bearing or mechanically demanding applications. To further demonstrate the geometric versatility of the material, a representative inner ear geometry was fabricated via 3D printing. The printed structure highlights the ability of the conductive foam to replicate complex, anatomically relevant shapes (Figure S2). Importantly, electrical conductivity measurements revealed that the 3D‐printed foams exhibit conductivities (3.48 × 10−4 ± 5.36 × 10−5 S cm−1) comparable to those of the corresponding hot‐pressed 75% void‐fraction foams (6.84 × 10−4 ± 2.60 × 10−5 S cm−1), indicating that the extrusion and printing steps do not disrupt the percolated PEDOT:PSS network. This preservation of electrical performance confirms that the conductive pathways formed by the coated microspheres remain intact throughout filament fabrication and printing. Overall, the low variability in mechanical testing demonstrates that the materials and 3D printing approach enable scalable, repeatable fabrication of electrodes with tunable mechanical and electrical properties. This positions the developed syntactic foams as promising platforms for bioelectronic devices, where reliable strength, flexibility, and processability are essential for future development. Chemical and Physical Recycling To evaluate the recyclability of the composite foams, a chemical separation method was implemented to isolate and recover the conductive PEDOT:PSS‐coated microspheres from the PCL matrix (Figure 7a). The foams were first cut into small pieces and submerged in ethyl acetate, a green solvent that selectively dissolves PCL while leaving the microspheres intact. After complete dissolution of the polymer matrix, the suspension was filtered through a stainless‐steel mesh to physically separate the microspheres from the polymer solution. The recovered microspheres were deposited onto a Kapton substrate and heated at 70 °C to remove residual solvent. The integrity of the PEDOT:PSS coating following the recycling process was examined by SEM. The images confirmed that the microspheres remained coated with the conductive polymer, with no sign of aggregation, cracking, or delamination. This indicates that the solvent treatment and mild heating did not visibly damage the conductive coating. Importantly, this chemical process is intended to demonstrate recovery of the conductive microsphere component from the PCL matrix, rather than complete closed‐loop recycling into the identical device. (a) Chemical recycling of the foams via dissolution of the PCL matrix, allowing recovery of PEDOT:PSS‐coated microspheres for reuse in new formulations. (b) Physical recycling through the melting and reshaping of the foam into new geometries. (c) Optical microscope images showing the time‐lapse progression of defect closure in a punctured foam during thermally assisted repair (0–20 s), demonstrating rapid defect closure upon localized heating. In parallel, physical recycling was explored by mechanically cutting used foams into small fragments and reprocessing them through hot pressing. The fragments were successfully reshaped into uniform films and cubes without visible degradation, delamination, or cracking (Figure 7b). This route exploited the thermoplasticity of PCL, enabling reshaping while preserving the distribution of conductive microspheres. As shown in Figure S3a, the compressive modulus of the foams remains within the same range after the first and fifth recycling cycles, indicating negligible mechanical degradation. In addition, time‐dependent current measurements (Figure S3b) reveal stable electrical responses across recycling cycles, confirming the preservation of conductive pathways upon repeated reprocessing. Tensile stress‐strain behavior remains largely unchanged after recycling, further confirming a good retention of mechanical performance (Figure S3c). SEM imaging after five recycling cycles shows that the porous microstructure is preserved, suggesting that the overall foam architecture is maintained during reprocessing (Figure S3d). Furthermore, DSC thermograms of the original material and after five recycling cycles show no significant changes in thermal transitions (Figure S3e), indicating that the thermal properties remain stable during reprocessing. Together, these results demonstrate that the foams can be thermally reprocessed while retaining structural and functional integrity under the tested conditions. In addition, selective dissolution of the PCL matrix enables recovery of the conductive microsphere component, providing a practical route to extend material service life. The thermally assisted repair capability of the foam was demonstrated by intentionally puncturing a film (thickness of ∼5 mm) with a sewing needle and then applying localized heat to facilitate repair (Figure 7c). Various heat sources, including a hot plate, hot press, oven, or heat gun, can be used to trigger thermally assisted repair. In this experiment, a heat gun was directed at the punctured foam for 20 s, during which a series of images captured the gradual closure of the defect (Video S1). The surface temperature during heating ranged between 80 °C and 100 °C (depending on the distance between the heat source and the sample), exceeding the melting temperature of the polymer matrix. Under these conditions, the thermoplastic PCL matrix softens and undergoes localized melting and reflow, enabling polymer chain interdiffusion across the damaged interface and re‐solidification upon cooling. Importantly, the embedded conductive microspheres remain intact during this process, allowing the conductive network to be preserved after repair. This thermally assisted repair demonstrates rapid morphological restoration of localized structural defects and is particularly relevant for wearable devices, where minor mechanical damage, such as punctures or cuts, can be closed through localized thermoplastic reflow to help maintain device integrity and extend service life. Electrophysiological Signal Recording To demonstrate the proof‐of‐concept applicability of the developed conductive foams, we fabricated an epidermal electrode using the optimized 85% void‐fraction foam and evaluated its performance for epidermal biosensing. The foam electrode was integrated into a standard snap‐type configuration and used to record physiological signals, including electrocardiography (ECG) and electromyography (EMG). Representative ECG recordings clearly resolve characteristic P‐QRS‐T waveforms with stable amplitudes and low baseline noise (Figure S4a), while EMG measurements exhibit distinct, repeatable bursts corresponding to voluntary muscle activation (Figure S4b). These results confirm that the porous conductive foam provides reliable skin‐electrode contact and sufficient electrical performance for high‐fidelity acquisition of epidermal bioelectrical signals. Brain electrical activity can be recorded noninvasively using electroencephalography (EEG), a proven technique widely employed in both clinical diagnostics and cognitive monitoring [58, 59]. Among the different EEG rhythms, alpha‐band oscillations in the 8–13 Hz range are closely associated with relaxed wakefulness and are commonly used as benchmarks for assessing signal quality [60, 61] While conventional EEG systems rely on scalp‐mounted, clinician‐dependent and highly disruptive electrode caps, recent work has highlighted the ear canal as a particularly attractive sensing site due to its close anatomical proximity to the central nervous system and its potential for unobtrusive, long‐term monitoring [9, 62, 63, 64, 65]. A comprehensive review of electrode materials and form factors for scalp, around, and in‐ear EEG was conducted by the authors and published [59]. It outlined key design requirements for wearable ear‐EEG systems, which could all be met with conformable conductive foam. The ear‐EEG device developed here is entirely foam‐based and ultralight, which allows it to be worn comfortably for extended periods of time during everyday activities. The compliant foam structure enables effortless insertion into the ear canal and adapts to its unique geometry, promoting close‐range, stable yet inconspicuous contact with the skin (Figure 8a,b). This combination of conformability and low mechanical burden makes the platform well‐suited for long‐term in‐ear EEG sensing outside of laboratory and clinical constraints. (a) Schematic of the foam‐based in‐ear EEG electrode. Schematic created with BioRender. (b) Illustration and photograph of electrode placement for ear‐EEG recording, including reference (Ref) and ground (GND) electrodes. (c) Experimental protocol for eyes open (O) and eyes closed (C) conditions. (d) Time‐frequency spectrogram of the EEG signal showing power distribution across frequencies. (e) Temporal evolution of alpha‐band (8–12 Hz) activity. Dashed lines indicate one episode of the eyes‐closed condition. Time‐frequency analysis of in‐ear EEG recordings demonstrates the foam‐based electrode's ability to capture physiologically meaningful brain rhythms (see Supporting Information for full signal analysis). The eyes‐open/eyes‐closed (EOEC) paradigm is widely recognized as an initial validation test to ensure new EEG systems are recording brain activity. The paradigm is simple, robust, and alpha modulation is well‐characterized [66, 67, 68]. A single in‐ear channel was recorded continuously over alternating 20 s blocks of eyes‐open and eyes‐closed (Figure 8c) while the subject remained seated and relaxed. The spectrogram (Figure 8d) shows clear power modulation in the alpha band (8–12 Hz) over time, with repeated increases in alpha activity corresponding to periods of eye closure and attenuation during eye opening, as indicated by the experimental protocol. This expected alternation between eyes‐open and eyes‐closed alpha activity is a well‐established EEG hallmark and confirms that the in‐ear foam electrode can reliably detect dynamic changes in actual cortical activity. To quantify this behavior, the temporal evolution of alpha‐band power was extracted and is shown in Figure 8e. The alpha activity exhibits consistent and repeatable fluctuations aligned with the task sequence, further supporting stable electrode‐skin contact and low susceptibility to motion‐related artifacts during the recording. Collectively, these observations indicate that the foam‐based in‐ear electrode supports reliable extraction of both temporal and spectral EEG features associated with relaxed wakefulness. Conclusion In summary, we have developed a class of recyclable and 3D‐printable conductive syntactic foams based on PEDOT:PSS‐coated polymer microspheres embedded in a thermoplastic matrix. By localizing conductivity at the microsphere surface, this architecture enables simultaneous control over porosity, mechanical compliance, and electrical performance while preserving low density and scalable processability. Importantly, microsphere‐templated conductive shells provide a materials design strategy that decouples electrical functionality from bulk polymer loading, overcoming limitations commonly encountered in conventional conductive foams. Beyond performance, these materials introduce practical routes toward circular soft electronics. The foams can be reprocessed through both chemical recycling, via selective matrix dissolution and microsphere recovery, and physical recycling through thermal reshaping, without loss of structural integrity or conductivity. Compatibility with fused filament fabrication further enables rapid prototyping and geometric versatility using standard additive manufacturing tools. Demonstrated here in soft wearable electrodes for electrophysiological signal acquisition, including in‐ear EEG, this work establishes conductive syntactic foams as a versatile and sustainable materials platform. More broadly, the microsphere‐templated approach outlined here offers a general framework for designing lightweight, compliant, and recyclable functional materials for next‐generation soft and wearable electronic systems. While the present study demonstrates the feasibility of additive manufacturing using this material system, further work is needed to systematically investigate the influence of printing parameters and to extend printability to higher void fraction foams. In addition, a more comprehensive evaluation of long‐term stability and device performance under operational conditions will be important. Although the present study demonstrates proof‐of‐concept skin and in‐ear electrophysiological recording, the long‐term skin and ear‐contact safety of the final PCL/PEDOT:PSS/microsphere foam remains to be established. Such efforts will help fully leverage the mechanical compliance and lightweight nature of these materials in complex device geometries. Experimental Section/Methods Materials Poly(4‐styrenesulfonic acid) sodium salt (PSS), 3,4‐Ethylenedioxythiophene (EDOT), ammonium persulfate (APS), and hydrochloric acid (HCl) were purchased from Millipore Sigma (St. Louis, MO, USA) and used as received. Expanded hollow microspheres (Expancel grade 920 DE 40 d30, particle size 35–55 µm, density 27–33 kg m−3) were supplied by AkzoNobel, Duluth, GA, USA. Poly(ε‐caprolactone) (PCL, CAPA 6500; density 1.02 g cm−3; melt flow index of 7 g 10 min−1; melting point 58–60 °C) was supplied by Ingevity, USA. PEDOT:PSS (Clevios PH1000 aqueous suspension; PEDOT:PSS content 1‐1.3%) was purchased from Heraeus Precious Metals (Germany). Ethyl acetate was purchased from VWR (Radnor, PA, USA). For simplicity, uncoated hollow microspheres are referred to as MS (microspheres), while the PEDOT:PSS‐coated conductive microspheres are denoted as CMS (conductive microspheres) throughout this work. Microsphere Preparation To coat Expancel microspheres with PEDOT:PSS, 15 mL of 1 wt.% PSS sodium salt solution in DI water was first prepared, followed by the addition of 1 mL of 1 M HCl. Next, 50 mg of Expancel microspheres were dispersed in the prepared PSS‐HCl solution, which was sonicated for 5 min to ensure complete wetting of microsphere surfaces. Subsequently, 50 µL of EDOT monomer was added to the dispersion, which was stirred gently without oxidant for 60 min at room temperature to promote EDOT adsorption onto the microsphere surfaces. The oxidant solution, prepared by dissolving 70 mg of APS in 10 mL of DI water, was then added dropwise to the Expancel suspension over 30 min under gentle stirring to initiate in situ oxidative polymerization on the surface of the MS. The reaction mixture was then covered with aluminum foil and left to polymerize at room temperature under gentle stirring. This PEDOT:PSS synthesis procedure was adapted from prior reports [69, 70] with modifications to accommodate microspheres as the template. To investigate the effect of polymerization duration, samples were prepared with reaction times of 2, 4, 8, 12, and 24 h under otherwise identical conditions. During polymerization, the solution gradually changed color from white to dark blue, which is characteristic of PEDOT:PSS formation and indicates the increase in the coating thickness with reaction time. The reaction was terminated by adding 5 mL of methanol to quench the polymerization. The mixture was sieved through a 500‐mesh screen to collect the coated microspheres, which were thoroughly washed with DI water to remove residual reagents. The microspheres were subsequently dried at room temperature for 24 h, then passed through a 300‐mesh screen to break apart agglomerates. The resulting powder was collected as the final conductive microsphere (CMS) product. For comparison, a conductive microsphere powder was also prepared by physically mixing uncoated Expancel microspheres with PH1000. Microspheres and PEDOT:PSS dispersion were combined precisely in a 1:3 weight ratio (microspheres:PH1000) and hand‐mixed with a spatula until a homogeneous paste‐like consistency was obtained. The mixture was spread onto a Kapton film and dried in an oven at 80°C for 4 h. The dried film was carefully scraped from the substrate, sieved through a 300‐mesh screen to remove aggregates, and processed into a fine, uniform powder. This powder was used in foam fabrication as a control material to benchmark against the in situ PEDOT:PSS‐coated microspheres produced via the synthesis route. The density of the conductive powder was measured using a Micromeritics AccuPyc II 1345 gas pycnometer (Norcross, GA, USA) equipped with a 10 cm3 sample cell, where helium gas displacement was used to determine the sample volume and calculate its density. Particle size distribution was determined using a LA‐950 laser diffraction analyzer (HORIBA Instruments, Irvine, CA, USA). Briefly, a small amount of powder was dispersed in deionized water, the suspension was gently homogenized and ultrasonicated to minimize agglomeration, and then introduced into the instrument for measurement. Foam Preparation Conductive foams were fabricated by a solution‐casting method. PCL pellets were dissolved in ethyl acetate at room temperature using a magnetic stirrer. PCL and ethyl acetate were selected by virtue of their biodegradability, low toxicity, and compatibility with low‐temperature processing, enabling an energy‐efficient and environmentally conscious fabrication route [71, 72]. Once PCL was completely dissolved, the CMS powder was added to the solution and mixed to form a viscous slurry. The void fraction of the foam, defined as the ratio of the volume of void space to the total foam volume, was controlled by adjusting the volume ratio of microspheres to PCL, with higher CMS content yielding greater void fraction. The slurry was ultrasonicated with Branson 2510 Ultrasonic Cleaner (70 W) at 40°C for 10 min and then dried in a Thermo Scientific Heratherm oven for 5 h at 50°C to remove residual solvent. Finally, the dried samples were molded into the desired shapes by pressing them at 100°C under an applied pressure of approximately 190 kPa using a heat press (Combo heat press machine). The pressing time was adjusted between 1 and 5 min depending on the sample size and thickness. After pressure release, the samples were allowed to cool in the mold for 10 min before demolding. The foam density was determined by measuring the mass of 3 cuboidal specimens (∼10 × 10 × 10 mm), dividing each by its respective volume, and reporting the average values for each sample type. A puncture test was performed by manually piercing the film through its full thickness using a standard sewing needle, followed by immediate needle removal. Images were taken using a digital microscope (Dino‐Lite Edge 3.0 AM73915MT8, USA). The healing was triggered by a hot air gun (SEEKONE Heat Gun SDL‐2816). The surface temperature during heating ranged from 80 to 100°C, depending on the distance between the heat source and the sample. Thermogravimetric analysis (TGA, 5500, TA Instruments, USA) was performed on both CMS and foams to evaluate their thermal stability. Measurements were performed in an open platinum crucible from 40–600°C with a heating rate of 20°C min−1, under a nitrogen atmosphere (40 mL min−1). Additionally, differential scanning calorimetry (DSC, Q2000, TA Instruments, USA) was conducted to study the thermal properties of the foams. 5–10 mg of samples were placed in a closed‐lid standard aluminum pan and subjected to nitrogen flow. To remove the influence of prior thermal history and obtain a reliable representation of the intrinsic thermal behavior, the samples were initially cooled to 0°C and heated to 250°C at a rate of 10°C min−1. A second heating cycle was then carried out under the same conditions, from 0°C to 150°C at 10°C min−1, and the data from this second run were used for analysis. Scanning Electron Microscopy (SEM) The morphology of the foams was examined using a Quattro (Thermo Scientific) scanning electron microscope (SEM) equipped with an energy‐dispersive spectrometer (EDS). The CMS powder was manually spread onto adhesive carbon tape (commonly used for SEM sample mounting) using gentle fingertip pressure to ensure uniform surface coverage. The foams were cryo‐fractured using liquid nitrogen to achieve a clean representative cross‐section of their internal structure. Mechanical and Electrical Characterization Mechanical tests were performed using a Mach‐1 V500csst MA009 mechanical tester (Biomomentum Inc., Canada) equipped with a 250 N load cell. Compression tests were performed on cubic specimens (10 × 10 × 10 mm) at a compression rate of 0.1 mm s−1. A flat circular indenter with a diameter of 32 mm was used. Prior to testing, all samples were hot‐pressed at 100°C in molds to achieve the desired shapes. Electrical conductivity measurements were carried out using a tailored tensile grip with electrodes (model MA068, Biomomentum Inc., Canada), interfaced with a source measure unit (B2902A, Agilent). The conductivity (σ) of the films was determined as follows: (1) σ=LR×A where R denotes the average resistance, and L and A are the length and cross‐sectional area of the foams between two grips, respectively. The reported conductivity values correspond to the average of 3 measurements, with error bars representing the standard deviation. To validate the uniformity and repeatability of the 3D printing process, tensile tests were conducted on printed dogbone specimens prepared according to the testing standard ASTM D638 Type V, using an Instron 3365 universal testing machine (Norwood, MA) with a 500 N load cell. The tests were performed at a crosshead displacement rate of 10 mm s−1. Each measurement was repeated at least four times to ensure consistent evaluation of the mechanical performance across samples. Fourier‐Transform Infrared (FTIR) Spectroscopy Fourier‐transform infrared (FTIR) spectroscopy was performed in absorption mode using a PerkinElmer Spectrum 65 spectrometer. A background spectrum was obtained prior to sample measurement. Spectra were acquired at room temperature over the range of 4000–600 cm−1 with a resolution of 4 cm−1, across 32 scans per measurement. The powder samples were placed directly onto the ATR crystal for measurement without additional preparation. Each sample was analyzed three times under identical conditions. For the PEDOT:PSS reference spectrum, the PEDOT:PSS dispersion was drop‐casted onto a clean glass slide, dried at room temperature to form a free‐standing film, and subsequently analyzed under identical conditions. Additive Manufacturing The foams were additively manufactured via the Fused Filament Fabrication (FFF) method. As depicted in Figure 9, the process includes the fabrication of filaments via an extruder (Figure 9a) and then the deposition of molten filaments layer by layer via a 3D printer (Figure 9b). Pure PCL and solution‐cast foams with a 75% void fraction were cut into pellets (about 5 × 5 mm) for filament extrusion. The pellets were gravity‐fed into a single‐screw extruder (3Dpany Extruder, with screw diameter of 20 mm and length‐diameter ratio of L/D = 15:1), where they were conveyed and melted under controlled heating. Schematic illustration of (a) foam pellet extrusion into filaments and (b) fused filament fabrication (FFF) 3D printing. Schematic created with BioRender. To preserve the microspheres, the heating temperatures (listed in Table 2), mainly determined by the melting temperature of PCL (∼60°C), are relatively low compared to those of commonly used FFF filaments, such as polylactic acid (PLA, printing temperature of 190 °C). The molten material was pushed through a circular die with a diameter of 1.75 mm under coordinately controlled screw speed and traction speed, which determine the production rate and adjust filament diameter, to produce continuous filaments suitable for commercial 3D printers. The hot extrudate was cooled by directed airflow at different fan speeds to stabilize its geometry while avoiding brittleness or deformation. Cooled filaments were then collected by a synchronized winding system that maintained constant tension and ensured uniform filament diameter. Table 1 shows the processing parameters used for PCL and foam filament fabrication. The diameters of the filaments were obtained by averaging the measurements taken at five different positions. TABLE 2Processing parameters of the single‐screw extruder.SampleCompression Zone Temperature (°C)Nozzle Temperature (°C)Screw Speed (rpm)Traction Speed (mm/s)Fan Speed (%)Average Filament Diameter (mm)PCL708541.3701.76 ± 0.04Foam7390121.31001.73 ± 0.04John Wiley & Sons, Ltd. Processing parameters of the single‐screw extruder. A Bambu Lab A1 mini 3D printer was used to fabricate both foamed filaments with 75% void fraction and benchmarking PCL samples (via filaments of 1.75 mm diameter). A hotend with a nozzle diameter of 0.8 mm was utilized to alleviate flow resistance and avoid clogging. Bambu Studio slicing software was employed to convert the 3D digital models into layered printing instructions. The key processing parameters used for 3D printing are summarized in Table 3. The nozzle temperature was selected based on printability and material stability. For the foam material, printing was intermittent below 170°C, while higher temperatures led to degradation and adhesion to the nozzle. Accordingly, a nozzle temperature of 170°C was used. A relatively low printing speed was selected to maintain surface quality, as higher speeds led to noticeable defects. The bed temperature was set to 30°C, as thermal stresses in soft materials are minimal, and adhesion to the build platform was sufficient at near‐room temperature. Full infill (100%) was used to obtain mechanically robust specimens. A layer height of 0.5 mm was selected. The building orientation was defined as the horizontal direction (0°) being parallel to the hotplate, and the vertical direction (90°) being perpendicular to the hotplate (Figure 6d). The default setting in the Bambu Studio slicing software (e.g., ± 45°) was taken as the raster direction. Tensile loading directions are parallel to the building orientation. As a unified material system, the proposed foams at different void fractions are 3D printable (refer to Figure S5 for details on additive manufacturing of the 85% void fraction foam). The proposed foams are FFF‐compatible under the aforementioned processing conditions. Due to the fact that this article is unable to conduct extensive tests covering all process parameters on the proposed foam for FFF additive manufacturing, the comparison of printed and hot‐pressed foams of the same void fraction by SEM, density, conductivity, and tensile properties will be conducted in future comprehensive studies on processing conditions TABLE 3Processing parameters of the 3D printing via the FFF method.SampleNozzle Temperature (°C)Printing Speed (mm/s)Bed Temperature (°C)Infill Density (%)Line Width (mm)PCL19015301000.78Foam17010301000.78John Wiley & Sons, Ltd. Processing parameters of the 3D printing via the FFF method. Electrophysiological Signal Recording Electrophysiological recordings, including electrocardiography (ECG), electromyography (EMG), and electroencephalography (EEG), were performed on one healthy volunteer to evaluate the performance of the developed electrodes in representative biosensing applications. All measurements were conducted on a healthy volunteer, and signals were acquired using a biosensing board (Cyton, OpenBCI, USA) at a sampling rate of 250 Hz. Foams with an 85% void fraction were cut into disks (8 mm diameter, 5 mm thickness). Electrical contacts were established using silver (Ag) traces connected to the snap button of a commercial Ambu electrode (Figure S6a). These assemblies were used for ECG and EMG measurements, and additionally as reference and ground electrodes in EEG recordings. ECG signals were recorded using a standard limb‐lead configuration (Figure S6b). The ground and positive electrodes were placed on the left forearm, while the negative electrode was positioned on the right forearm. The electrodes were connected to the biosensing monitor, and cardiac signals were recorded in real time. During acquisition, a bandpass filter of 5–50 Hz was applied, along with a 60 Hz notch filter to suppress power‐line interference. Offline signal processing was performed using a second‐order digital Butterworth high‐pass filter with a cutoff frequency of 0.5 Hz to remove baseline drift. Surface EMG measurements were conducted on the flexor carpi muscle of the right forearm (Figure S6c). Three electrodes were placed along the muscle. EMG signals were recorded while the participant performed repeated voluntary hand and wrist flexion–extension movements for durations of 1–2 s. Data acquisition was carried out with a bandpass filter of 15–50 Hz. Offline processing involved applying a second‐order digital Butterworth high‐pass filter with a cutoff frequency of 10 Hz to eliminate baseline drift. Ear‐EEG measurements were performed using the developed 85% void‐fraction conductive foam electrode, integrated onto a commercial Onhear foam earplug to enable in‐ear recording (Figure 8a and Figure S6d). The foam electrode (15 mm × 15 mm) was glued onto the foam base of the earplug to ensure conformal contact with the ear canal. The recording electrode was positioned within the ear canal, with a reference electrode placed on the ipsilateral mastoid and a ground electrode attached to the earlobe (Figure 8b). EEG signals were acquired during a 10 min recording session. Brain activity was analyzed in the 0–25 Hz frequency range, with particular emphasis on alpha‐band activity (8–12 Hz), a hallmark of relaxed wakefulness (see Supporting Information for full signal analysis). Author Contributions Gayaneh Petrossian: Conceptualization, Methodology, Investigation, Writing – original draft. Yassine Diouri: Methodology. Bolan Xu: Methodology, Data curation. Sara Ebrahimi: Methodology, Writing – review & editing. Atharva Pande: Methodology. Floriane Miquet‐Westphal: Methodology, Writing – review & editing. Hang Xu: Methodology, Conceptualization, Writing – review & editing, Writing – original draft, Supervision, Investigation. Fabio Cicoira: Supervision, Conceptualization, Investigation, Funding acquisition, Project administration, Writing – review & editing, Writing – original draft, Methodology Funding This research was supported by the Natural Sciences and Engineering Research Council of Canada (NSERC) through Discovery Grants awarded to FC (grant No. RGPIN‐2025‐05607) and HX (grant No. RGPIN‐2024‐06567). The equipment and infrastructure used in this study were acquired and maintained by the Canada Foundation for Innovation, FRQNT, and NSERC. GP acknowledges support from the NSERC Vanier Canada Graduate Scholarship. Y.D. acknowledges support from CREPEC for the Complément de bourse (Maitrise) scholarship. S.E. and F.M.W. acknowledge the Fonds de recherche du Québec—Nature et technologies (FRQNT) for a Doctoral Scholarship. BX acknowledges support from NSERC Undergraduate Student Research Award (USRA). Conflicts of Interest The authors declare no conflict of interest. Supporting information Supporting File 1: adhm71364‐sup‐0001‐SuppMat.docx. Supporting File 2: adhm71364‐sup‐0002‐VideoS1.mp4.