Mechanically adaptive crack-resistant hydrogels based on strain-induced macroscopic phase separation and hierarchical energy dissipation Authors: Xiangren Kong, Zhongwei Wang, Bo Gong, Li Xin Hou, Zhi Jian Wang, Rui Xiao, Zi Liang Wu, Jin Qian Published: 2026 ABSTRACT It remains a significant challenge to simultaneously achieve high stiffness, large extensibility, and strong resistance to crack propagation in hydrogels. Here, we report a hydrogel that undergoes a fully reversible strain-induced whitening transition with a high modulus ( ~ 30 MPa), high tensile strength (~15 MPa), large stretchability ( > 1000%). Importantly, the hydrogel achieves an exceptional fracture toughness around 100 kJ m−2 and exhibits the ability to autonomously suppress crack growth under load. The hydrogel is constructed from a strong polycation and a weak polyanion at an asymmetric molar ratio, producing a transparent and initially isotropic network containing ionic-bond-rich and hydrogen-bond-rich nanodomains. In situ X-ray scattering measurements, combined with molecular dynamics simulations, reveal a multiscale structural transition under tensile deformation. Specifically, yielding of the hydrogen-bond-rich soft domains enhances interdomain contrast, inducing whitening, together with orientation and adaptive dissociation of ionic-bond-rich domains. This process forms an extended anisotropic dissipative zone, thus effectively blunting and arresting cracks. This work demonstrates how compositional asymmetry enables a macroscopically uniform and transparent hydrogel to autonomously evolve anisotropic energy-dissipation pathways under strain, providing an efficient strategy for creating damage-tolerant soft materials for extreme mechanical environments. Introduction Hydrogels have emerged as a vital class of soft materials for human-machine interfaces1, soft robotics2,3, tissue engineering4–6, and flexible electronics7,8, owing to their exceptional structural programmability and biocompatibility. For such applications, mechanical robustness, manifested as high modulus, strength, and stretchability, is crucial for maintaining performance under complex mechanical loads. However, these mechanical attributes are often mutually constrained9. For example, conventional single-network hydrogels typically exhibit brittle or weak behavior, reflecting the long-standing trade-off between stiffness and toughness, or equivalently, between crack resistance and deformability10. Achieving a simultaneous enhancement of these key properties remains a central challenge in hydrogel science. To achieve tough hydrogels, numerous toughening strategies have been proposed in the past decades, including the incorporation of sacrificial bonds11, nanoparticle fillers12, and crystalline or physically confined structures13,14. These architectures can effectively dissipate energy under large deformation and enhance fracture energy, albeit at the cost of irreversible damage and permanent loss of function. Hydrogels utilizing reversible interactions such as hydrogen bonding15, ionic association16, or host-guest complexation17, can recover their structure and performance to some extent. However, these materials typically remain vulnerable to stress concentration at crack tips, leading to catastrophic fracture under large stress. Crack insensitivity is essential for reliable operation under complex loading conditions, as hydrogels invariably encounter sharp defects and stress concentrators during service. A variety of mechanisms have been explored to resist crack propagation, including macroscopic chain orientation18, force-induced crystallization19, directional freezing20, fiber reinforcement21, secondary-network polymerization22,23, chain entanglement24, sequential crosslinking22,25, cyclic heating/cooling26,27, solvent exchange28, or nanoscale confinement polymerization29. Although these strategies significantly improve fatigue resistance, they typically rely on anisotropic microstructures and multi-step fabrication, and severe stress localization under large strain still triggers rapid crack growth. Photocoupling-based crosslinking strategies have enabled faster fabrication and improved interphase stress transfer30, yet the rigid and poorly deformable hard domains in these systems limit their ability to resist crack propagation. Hence, developing an intrinsically isotropic and strain-adaptive mechanism that can effectively suppress crack propagation persists as a critical challenge11,31–33. Inspired by the hierarchical architectures and adaptive energy-dissipation mechanisms of biological tissues34–36, we introduce a class of hydrogels constructed by complexing a strong cationic polyelectrolyte with a weak anionic component at a markedly asymmetric feed ratio. This asymmetric molecular design breaks the conventional requirement for strict charge stoichiometry in polyion-complex (PIC) hydrogels, yielding a transparent gel with nanoscale ionic-bond-rich and hydrogen-bond-rich domains. During uniaxial stretching, the hydrogel undergoes a continuous transition from yielding to strain hardening, accompanied by pronounced macroscopic whitening. In situ ultra-small-angle X-ray scattering (USAXS) and molecular dynamics simulations reveal that the whitening originates from the rapid deformation of hydrogen-bond-rich domains and the delayed deformation of ion-rich domains, which increase the density contrast and drive strain-induced macroscopic phase separation of the pre-existing heterogeneous network. At high strains, the naturally interpenetrated architecture enables efficient stress transfer between the two phases. The ionic-bond-rich domains continue to dissipate energy through ionic bond dissociation and chain alignment, forming crack arrestors oriented along the stretching direction. Benefiting from this cooperative energy-dissipation mechanism, the hydrogel achieves a high modulus (~30 MPa), high tensile strength (~15 MPa), and ultrahigh fracture toughness (~100 kJ m−2). This design provides a simple yet general strategy for achieving synergistic enhancement of stiffness, strength, toughness, and crack resistance under simplified fabrication conditions, offering insights into the rational design of mechanically robust soft materials. Results Hydrogel preparation, strain-induced whitening, and crack resistance Hydrogels were fabricated by complexing a strong polyelectrolyte, poly methacrylatoethyl trimethyl ammonium chloride (PMATAC), with a weak polyelectrolyte, polyacrylic acid (PAAc), using markedly asymmetric monomer feed ratios, for example, MATAC:AAc\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\,=\,$$\end{document}=1:3–1:5. Fourier-transform infrared (FTIR) spectroscopy confirmed the coexistence of ionic and hydrogen bonding interactions between the two polymers. The characteristic C=O stretching band at 1716 cm−1 red-shifted to 1710 cm−1, indicating the formation of hydrogen bonds between PMATAC and PAAc chains, while the emergence of intense peaks at 1558 and 1402 cm−1 corresponded to the asymmetric and symmetric stretching of –COO⁻ groups, confirming ionic complexation (Supplementary Fig. 1). Previous studies have suggested that polyion-complex (PIC) hydrogels tend to form contracted and segregated microstructures11. Given the relatively low PMATAC content (~20%), the resulting hydrogels naturally developed dispersed ion-rich domains embedded in a continuous hydrogen-bond-rich matrix (Fig. 1A). Nano-IR mapping at 1558 cm−1 revealed spatially isolated ionic-bond-rich domains (Fig. 1B), while hydrogen bonds (1710 cm−1) were distributed densely and uniformly throughout the matrix (Supplementary Fig. 2). Notably, even with two-phase domains, the gel preserves >90% optical transparency (Supplementary Fig. 3), a property crucial for many optical and biointegrated applications.Fig. 1Compositionally asymmetric polyelectrolyte hydrogel converts pre-existing heterogeneity into a macroscopically visible whitening state for crack suppression.A Schematic of the hydrogel design based on markedly asymmetric monomer feed ratios (MATAC:AAc = 1:3–1:5), producing a transparent network with dispersed ion-bond-rich (hard phase) and hydrogen-bond-rich (soft phase) domains that share similar densities but have distinct noncovalent bond strengths. B Nano-IR mapping at 1558 cm−1 showing discrete ionic-bond-rich domains dispersed within the matrix. C Representative tensile stress–strain curve of the 1:3 gel, showing a transparent yield-like plateau at strains below the whitening threshold (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\varepsilon }_{w}$$\end{document}εw) and a subsequent strain-hardening regime accompanied by macroscopic whitening once the strain exceeds \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\varepsilon }_{w}$$\end{document}εw. Insets show representative optical appearances at different deformation stages. D Schematic illustration of the transparent stage at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\varepsilon=200\%$$\end{document}ε=200%, where the global strain remains below \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\varepsilon }_{w}$$\end{document}εw and the pre-existing heterogeneous domains are only weakly perturbed. E Schematic illustration of the whitening stage at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\varepsilon=600\%$$\end{document}ε=600%, where the strain exceeds \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\varepsilon }_{{w}}$$\end{document}εw and the pre-existing heterogeneous domains are further reorganized into macroscopically visible whitening regions. F Notched 1:3 hydrogel at a global strain of 200%. While most of the specimen remains transparent, a pronounced whitening zone nucleates only at the crack tip owing to local strain amplification, blunting the initially sharp notch and effectively hindering further crack advance. G Fracture toughness versus elastic modulus for this work compared with representative tough hydrogels, showing the combined high modulus (~30 MPa) and fracture toughness (~100 kJ m−2) achieved by the strain-adaptive polyelectrolyte network. Scale bars are 5 mm. Compositionally asymmetric polyelectrolyte hydrogel converts pre-existing heterogeneity into a macroscopically visible whitening state for crack suppression. A Schematic of the hydrogel design based on markedly asymmetric monomer feed ratios (MATAC:AAc = 1:3–1:5), producing a transparent network with dispersed ion-bond-rich (hard phase) and hydrogen-bond-rich (soft phase) domains that share similar densities but have distinct noncovalent bond strengths. B Nano-IR mapping at 1558 cm−1 showing discrete ionic-bond-rich domains dispersed within the matrix. C Representative tensile stress–strain curve of the 1:3 gel, showing a transparent yield-like plateau at strains below the whitening threshold (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\varepsilon }_{w}$$\end{document}εw) and a subsequent strain-hardening regime accompanied by macroscopic whitening once the strain exceeds \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\varepsilon }_{w}$$\end{document}εw. Insets show representative optical appearances at different deformation stages. D Schematic illustration of the transparent stage at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\varepsilon=200\%$$\end{document}ε=200%, where the global strain remains below \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\varepsilon }_{w}$$\end{document}εw and the pre-existing heterogeneous domains are only weakly perturbed. E Schematic illustration of the whitening stage at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\varepsilon=600\%$$\end{document}ε=600%, where the strain exceeds \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\varepsilon }_{{w}}$$\end{document}εw and the pre-existing heterogeneous domains are further reorganized into macroscopically visible whitening regions. F Notched 1:3 hydrogel at a global strain of 200%. While most of the specimen remains transparent, a pronounced whitening zone nucleates only at the crack tip owing to local strain amplification, blunting the initially sharp notch and effectively hindering further crack advance. G Fracture toughness versus elastic modulus for this work compared with representative tough hydrogels, showing the combined high modulus (~30 MPa) and fracture toughness (~100 kJ m−2) achieved by the strain-adaptive polyelectrolyte network. Scale bars are 5 mm. When stretched, the hydrogel exhibits a distinctive mechanical response characterized by a high initial modulus, a broad yielding plateau, and a pronounced strain-hardening regime (Supplementary Movie 1). The whitening threshold, \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\varepsilon }_{w}$$\end{document}εw, was defined as the abrupt change of the transmittance-strain curve, i.e., the intersection between the initial high transmittance regime and the subsequent steep-decline regime (Supplementary Fig. 4). For the 1:3 formulation, \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\varepsilon }_{{w}}$$\end{document}εw is approximately 400% and closely coincides with the onset of strain hardening after the yield-like plateau, linking the whitening transition to stress-activated structural reorganization within the network (Fig. 1C). SEM examination of samples fixed in the whitened state revealed no obvious pores in the whitened region (Supplementary Fig. 5). Further scattering comparison shows that, unlike cavitation-related patterns, our hydrogel exhibits an opposite 2D anisotropy and no cavitation-like low-q jump upon whitening (Supplementary Fig. 6), supporting a density-contrast origin rather than pore- or cavitation-driven whitening. Despite this drastic optical change, the material sustains exceptionally large deformations (>1000%) and achieves high tensile strength. Upon stretching, the densely distributed physical bonds and extensive chain entanglements provide a high modulus10,24. As deformation proceeds, weak hydrogen bonds and other labile interactions rupture first, leading to a yielding plateau in which the deformation is relatively uniform and the densities of the two phases remain comparable (Fig. 1D), thus maintaining transparency. When the stress starts to activate the strong ionic bonds or chain entanglements, strain hardening occurs. At this stage, the density of the hydrogen-bond-rich phase decreases rapidly, whereas the density of the ionic-bond-rich phase changes slightly, resulting in an increased density contrast and macroscopic whitening (Fig. 1E). Critically, the intimate interconnection between the two phases facilitates efficient stress transfer, thereby enhancing the stretchability and load-bearing capability of the gel37. As the ionic-bond-rich regions experience partial bond dissociation under the large transmitted load, their hard phase domains enlarge and become oriented along the tensile direction, forming crack arrestors that block crack propagation. Meanwhile, the strong interphase coupling promotes collective hardening of multiple PAAc chains31, leading to increase in the observed fracture strength. The whitening marks a transformation in the gel’s damage tolerance. In a notched sample, whitening nucleates only near the crack tip at a global strain of ~200%, while the surrounding material remains transparent (Fig. 1F and Supplementary Movie 3), indicating that local strain amplification enables the crack-tip region to exceed \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\varepsilon }_{w}$$\end{document}εw, thereby blunting the crack and suppressing catastrophic propagation. This self-organized protective zone arises without any predefined anisotropy, highlighting the intrinsically isotropic yet strain-adaptive nature of the network. As a result of this adaptive dissipation mechanism, the hydrogel achieves an exceptional combination of high modulus (~30 MPa), high tensile strength (~15 MPa), and ultrahigh fracture toughness approaching 100 kJ m−2 (Fig. 1G), exceeding the representative tough hydrogels9,10,38–42. Feed-ratio-governed mechanical response and whitening transition The tensile whitening is highly sensitive to the monomer feed ratio of the two polyelectrolytes (Supplementary Fig. 7A). Increasing the cation fraction mainly reduces the strength and modulus of the gel, whereas the effect on fracture strain is non-monotonic (Supplementary Fig. 7B). In particular, at PMATAC:PAAc\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\,=$$\end{document}=1:2.5, the gel shows a slightly higher fracture strain than the whitening formulations, but the tensile strength decreases by ~80% and the modulus by ~90%, and no whitening occurs during stretching (Fig. 2A). To probe the origin, we compared the rheology of whitening and non-whitening gels. The tensile-whitening composition (1:3.5) displays a double-peak in tan \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\delta$$\end{document}δ during temperature sweeps (Fig. 2B), indicating two phases with distinct relaxation mechanisms. In comparison, the non-whitening gel (1:2.5) exhibits a single tan \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\delta$$\end{document}δ peak over 0–80 °C (Fig. 2C), consistent with a uniform network at the observation scale. We attribute these differences to the excess cations in the 1:2.5 formulation: once the weak polyanion is saturated, additional cationic charges introduce electrostatic repulsion that lowers the effective binding energy of the network, thereby diminishing load-bearing capacity and suppressing whitening. Furthermore, the final water content of different proportions of hydrogels also varies (Supplementary Fig. 8), consistent with the trend of mechanical properties. This also reflects the strength of the internal bonding energy within the gel from a different perspective.Fig. 2Composition-dependent tensile response, viscoelastic transitions, stress relaxation, and whitening recovery of the hydrogels.A Representative tensile stress-strain curves for gels prepared with different MATAC:AAc monomer feed ratios, showing that the 1:2.5 formulation remains transparent, whereas strain-induced whitening emerges only at more asymmetric feed ratios, such as 1:3 and 1:3.5, together with increased strength and modulus but reduced fracture strain. B, C Temperature-sweep rheology: the whitening gel (1:3.5) exhibits a double tan \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\delta$$\end{document}δ peak, evidencing two phases with distinct relaxation mechanisms; the non-whitening gel (1:2.5) shows a single peak consistent with mechanical uniformity. D Stress-relaxation of the 1:3.5 whitening gel at fixed global strains: at 200% (transparent) and 500% (whitened), the stress drops to ~50% within ~10 s; over 500 s the residual stress decreases by ~80% and > 92%, respectively, indicating increased dissipation pathways in the whitened state. E Time-lapse images at 500% strain showing gradual and complete recovery of transparency over 6 h due to slow rebalance of dynamic bonds. F Color change of the 1:3 gel during a single loading-unloading process. G After reaching the yield platform stage, the load is removed from the 1:3.5 gel, initiating the self-recovery properties. H Upon unloading the 1:3.5 gel after being stretched to a state of intense whitening (near the fracture strain), the self-recovery processes of mechanical properties, as well as its color and dimensions, are shown (insets). Scale bars are 5 mm. Composition-dependent tensile response, viscoelastic transitions, stress relaxation, and whitening recovery of the hydrogels. A Representative tensile stress-strain curves for gels prepared with different MATAC:AAc monomer feed ratios, showing that the 1:2.5 formulation remains transparent, whereas strain-induced whitening emerges only at more asymmetric feed ratios, such as 1:3 and 1:3.5, together with increased strength and modulus but reduced fracture strain. B, C Temperature-sweep rheology: the whitening gel (1:3.5) exhibits a double tan \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\delta$$\end{document}δ peak, evidencing two phases with distinct relaxation mechanisms; the non-whitening gel (1:2.5) shows a single peak consistent with mechanical uniformity. D Stress-relaxation of the 1:3.5 whitening gel at fixed global strains: at 200% (transparent) and 500% (whitened), the stress drops to ~50% within ~10 s; over 500 s the residual stress decreases by ~80% and > 92%, respectively, indicating increased dissipation pathways in the whitened state. E Time-lapse images at 500% strain showing gradual and complete recovery of transparency over 6 h due to slow rebalance of dynamic bonds. F Color change of the 1:3 gel during a single loading-unloading process. G After reaching the yield platform stage, the load is removed from the 1:3.5 gel, initiating the self-recovery properties. H Upon unloading the 1:3.5 gel after being stretched to a state of intense whitening (near the fracture strain), the self-recovery processes of mechanical properties, as well as its color and dimensions, are shown (insets). Scale bars are 5 mm. We further performed stress-relaxation tests to understand network dynamics at different deformation stages (Fig. 2D). Two strains were selected: 200% (below \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\varepsilon }_{w}$$\end{document}εw, transparent yielding plateau) and 500% (above \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\varepsilon }_{w}$$\end{document}εw, whitened hardening regime). In both cases, the stress decays to around 50% within 10 s, reflecting rapid breakage/reformation of a large number of dynamic physical crosslinks-the primary source of yielding and toughness. Over 500 s, the transparent gel at 200% loses ~80% of its stress, while the whitened gel at 500% loses \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$ > $$\end{document}>92%, approaching negligible load-bearing. This indicates that whitening creates additional dissipation pathways: the entangled backbone and ionic-bond-rich domains are forced to stretch and align, forming a load-bearing skeleton during hardening; under fixed strain, these highly tensioned segments subsequently relax via ionic bond dissociation, disentanglement, and sliding, causing the pronounced stress decay. Maintaining 500% strain for 6 h leads to a gradual and ultimately complete recovery of transparency (Fig. 2E). This slow optical recovery indicates that the whitening state does not relax through simple viscoelastic relaxation alone, but instead involves slow structural/density re-equilibration between two physically crosslinked domains with distinct bond strengths. Over sufficiently long times, the dynamic bonds (particularly reversible ionic associations) reorganize and rebalance, allowing the oriented network to relax back to a macroscopically uniform transparent state. The tensile-whitening hydrogel exhibits pronounced reversibility. During unloading from a strain close to fracture, the whitened region progressively faded and nearly vanished (Fig. 2F and Supplementary Movie 1), supporting reversible concentration fluctuations between the two phases. Below the whitening threshold, the stress–strain response recovered within 1 h, implying rapid and reversible internal rearrangement (Fig. 2G). When stretched into the whitening regime, recovery was slower; nevertheless, the gel ultimately regained its dimensions, transparency and tensile response despite apparent yielding and strain hardening (Fig. 2H). This complete recovery indicates that the physical network preserves structural memory, without irreversible large-scale rearrangement of ionic associations or chain entanglements. Microstructural evolution during stretch-induced whitening The mesoscale structural evolution of the hydrogel during tensile whitening was elucidated by in-situ ultra-small-angle X-ray scattering (USAXS). Figure 3A shows the 2D scattering patterns at different deformation stages. The scattering images clearly reveal a transition from isotropic to anisotropic features as the strain increases (refer to the diagram at the bottom right corner). At low strain, or before the whitening threshold is reached, the SAXS pattern remains nearly isotropic and featureless, mainly because the scattering contrast between the coexisting soft and hard domains is still too low for the underlying heterogeneity to be clearly resolved43. Upon further stretching to the onset of whitening at Point 3 (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda \approx$$\end{document}λ≈3.5, corresponding to 250% engineering strain), the scattering becomes elliptical, with its major axis aligned with the tensile direction, implying the formation of transversely oriented heterogeneous structures44. This can be attributed to the smaller deformation of ionic-bond-rich domains compared with the hydrogen-bond-rich matrix, which compresses the lateral space and drives neighboring ionic-bond-rich regions to cluster, generating a laterally aligned morphology. As the stretch ratio \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda \approx \,$$\end{document}λ≈5.5, the scattering intensity increases markedly, indicating a growing density contrast between the rich and sparse phases. Enhanced scattering along the vertical direction suggests that structural orientation along the tensile axis results from elongation of the ionic-bond-rich domains as strong ionic bonds partially dissociate under increasing load. This produces laterally periodic spacing between adjacent domains. In contrast, the non-whitening gel exhibits isotropic diffuse rings throughout deformation (Fig. 3F), indicating the absence of pronounced phase amplification or long-range orientation, thereby confirming that the whitening behavior is associated with strain-induced macroscopic phase separation and anisotropy.Fig. 3In-situ USAXS characterization of the strain-induced structural evolution in the tensile-whitening hydrogel.A In-situ USAXS stress–strain curve and 2D scattering patterns showing transition from isotropic to anisotropic scattering with strain of the 1:3.5 gel. Among them, the lower right corner of the scattering patterns from point 3 to point 6 indicates the arrangement direction and degree of order of the internal heterogeneous structures. The arrow on the far right indicates the stretching direction. B 1D I(q) profiles integrated parallel to the tensile direction: high-q slope increases from 2.8 to 3.8 and a shoulder peak shift toward lower-q, indicating enhanced interface contrast and increased periodic spacing. C I(q) profiles perpendicular to the tensile direction: little change below \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 5.6; emergence of a low-q plateau and its shift to higher q at larger strain reflect vertical alignment and reduced spacing. D Gel-Fit model fitting of scattering data, yielding correlation length \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\xi$$\end{document}ξ and radius of gyration Rg as characteristic parameters of dense and sparse domains. E Extracted correlation lengths: parallel \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\xi$$\end{document}ξ increases from 85.8 nm to 174.1 nm, while vertical \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\xi$$\end{document}ξ decreases from 98 nm to 17.7 nm beyond \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 5.6. F In-situ 2D scattering patterns and 1D curves of the 1:2.5 non-whitening gel showing isotropic rings throughout stretching, indicating the absence of pronounced phase amplification or orientation. G In-situ WAXS patterns and integrated profiles revealing reduced interchain spacing and enhanced chain alignment with increasing strain. H AFM–IR absorption maps (1558 cm−1) showing ionic-bond-rich domains (red) become larger and more widely spaced after stretching, consistent with USAXS-derived evolution. Data are presented as mean ± s.d. (n ≥ 3). In-situ USAXS characterization of the strain-induced structural evolution in the tensile-whitening hydrogel. A In-situ USAXS stress–strain curve and 2D scattering patterns showing transition from isotropic to anisotropic scattering with strain of the 1:3.5 gel. Among them, the lower right corner of the scattering patterns from point 3 to point 6 indicates the arrangement direction and degree of order of the internal heterogeneous structures. The arrow on the far right indicates the stretching direction. B 1D I(q) profiles integrated parallel to the tensile direction: high-q slope increases from 2.8 to 3.8 and a shoulder peak shift toward lower-q, indicating enhanced interface contrast and increased periodic spacing. C I(q) profiles perpendicular to the tensile direction: little change below \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 5.6; emergence of a low-q plateau and its shift to higher q at larger strain reflect vertical alignment and reduced spacing. D Gel-Fit model fitting of scattering data, yielding correlation length \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\xi$$\end{document}ξ and radius of gyration Rg as characteristic parameters of dense and sparse domains. E Extracted correlation lengths: parallel \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\xi$$\end{document}ξ increases from 85.8 nm to 174.1 nm, while vertical \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\xi$$\end{document}ξ decreases from 98 nm to 17.7 nm beyond \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 5.6. F In-situ 2D scattering patterns and 1D curves of the 1:2.5 non-whitening gel showing isotropic rings throughout stretching, indicating the absence of pronounced phase amplification or orientation. G In-situ WAXS patterns and integrated profiles revealing reduced interchain spacing and enhanced chain alignment with increasing strain. H AFM–IR absorption maps (1558 cm−1) showing ionic-bond-rich domains (red) become larger and more widely spaced after stretching, consistent with USAXS-derived evolution. Data are presented as mean ± s.d. (n ≥ 3). The 2D scattering data were azimuthally integrated over 15° sectors parallel and perpendicular to the stretching direction to obtain 1D I(q) profiles (Supplementary Fig. 9), where q represents the magnitude of scattering vector, and I represents the scattering intensity. Figure 3B presents the parallel-direction results, revealing quantitative evolution of structural anisotropy. As strain increases, the high-q slope changes from ≈ 2.8 to ≈ 3.8, indicating sharpening of the interface between the dense and sparse domains45,46, i.e., an increasing density contrast. From \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 3, a shoulder appears and gradually shifts toward lower q, signifying an enlarged periodic correlation distance along the tensile direction14. Perpendicular profiles (Fig. 3C) remain nearly unchanged up to \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 5.6, and then display a low-q plateau that shifts to higher q with further stretching, reflecting the emergence of vertically oriented domains with reduced transverse spacing. For further quantitative analysis, the Gel-Fit scattering model47–49 was employed to fit the one-dimensional curve (Fig. 3D). The scattering profiles of the hydrogel were well captured by the model. The fitted coefficients and the corresponding fit quality, evaluated by the root-mean-square error in log10 I space, are summarized in two tables for the parallel and vertical datasets (Supplementary Table 1 and Table 2). The characteristic correlation lengths (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\xi$$\end{document}ξ) derived from the fitting are summarized in Fig. 3E. The yellow curve denotes the periodic spacing of laterally aligned heterogeneous domains, which gradually increases from 85.8 nm to 174.1 nm with strain, indicating that the two phases separate progressively along the tensile direction. In contrast, the vertical correlation length, which emerges at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 5.6, decreases from 98 nm to 17.7 nm, suggesting that the phases move closer perpendicular to the stretching axis. The radius of gyration (Rg), representing the size of the ionic-bond-rich domains, also evolves systematically. Along the tensile direction, Rg increases from 44.7 nm at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 3 to 67.4 nm at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 6.5, indicating elongation of the ionic-bond-rich regions under tension. In contrast, in the transverse direction (Supplementary Fig. 10), Rg decreases from 46 nm at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 5.6 to 33.5 nm at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 6.5, reflecting lateral contraction induced by stretching. Moreover, AFM-IR absorption mapping provides independent confirmation of this structural evolution. Before stretching, the separated ionic-bond-rich regions are ≈50 nm in size and spaced ≈100 nm apart (Fig. 3H, left). After stretching to \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 5, both the spacing and the domain size increase significantly (Fig. 3H, right), demonstrating that the ionic-bond-rich regions expand and move apart upon deformation. The characteristic size of these pre-existing heterogeneous domains is comparable in order of magnitude to the Rg (≈45 nm) resolved by USAXS at the onset of whitening, suggesting that the scattering objects emerging under load originate from the same domains. Thus, AFM-IR and USAXS provide complementary real-space and reciprocal-space views of the same structural evolution. Small-angle X-ray scattering (SAXS) was employed to probe finer structural features at the tens-of-nanometer scale. As shown in Supplementary Fig. 11, the 2D SAXS patterns of the tensile-whitening hydrogel exhibit elliptical contours oriented perpendicular to the stretching axis, even at small strains, indicating a rapid alignment of the polymer network at this length scale. The degree of orientation intensifies progressively with increasing strain, reflecting the continuous reorganization of the nanoscale network. In contrast, the non-whitening hydrogel maintains isotropic, diffuse ring patterns throughout deformation (Supplementary Fig. 12), demonstrating the absence of any pronounced orientation or phase separation. This contrast highlights the multiscale and hierarchical energy dissipation in the tensile-whitening hydrogel, whereas the non-whitening counterpart exhibits a single, uniform dissipation behavior. In addition, in-situ wide-angle X-ray scattering (WAXS) was performed to capture the structural evolution at the molecular scale (~1 nm) during stretching. As strain increases, the initially diffuse, isotropic scattering halo transforms into a broad circular ring, indicating that the intermolecular spacing evolves from a random distribution toward a more uniform distance (Fig. 3G). The integrated 1D profiles show a wide, shallow peak in the undeformed state, which gradually shifts to higher q and narrows upon stretching, signifying a decrease in interchain spacing and enhanced chain alignment. Notably, the in-situ WAXS results of the non-whitening hydrogel are nearly identical to those of the whitening gel (Supplementary Fig. 13), both exhibiting reduced interchain spacing upon strain and enhanced chain alignment. This indicates that reduced interchain spacing and chain entanglement, and alignment alone, are insufficient to account for the dramatic difference in crack resistance. All-atom molecular dynamics (MD) simulations during tensile deformation were used as a companion to the scattering experiments to probe the local structural reorganization underlying tensile whitening. To ensure consistency with the experimental feed ratios, the model preserves the relative degree-of-polymerization ratio of the polycation and polyanion inferred from the GPC analysis (Supplementary Fig. 14), while the absolute chain lengths were proportionally scaled down for computational feasibility. Accordingly, the simulations are intended to capture chemistry-specific local rearrangements and domain-level structural evolution, rather than the full entanglement-controlled macroscopic relaxation or fracture response of the experimental network50. The corresponding atomic configurations are provided in Supplementary Data. As shown in Fig. 4A, the cationic chains aggregated into discrete nanodomains within the anionic network. At \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 3, many anionic chains undergo significant elongation and the gel contracts laterally, while the less-deformable cationic clusters are compressed and forced to aggregate, as indicated by the red dashed regions, forming laterally aligned heterostructures on the sub−100 nm scale. At \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ= 6, the cationic clusters themselves are elongated, forming heterostructures aligned with the tensile direction.Fig. 4The mechanism of stretch-induced whitening and crack resistance.A All-atom molecular dynamics (MD) simulations reveal the evolution of microscopic structure during stretching, consistent with scattering observations. Among them, the PMATAC cluster was yellow, the PAAc cluster was blue, and the water molecules were gray. At \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 1, dispersed PMATAC clusters are embedded in the anionic matrix; at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 3, deformation of the anionic chains and lateral contraction compress the less-deformable cationic clusters, driving them to aggregate and form laterally aligned heterostructures (red dashed region); at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 6, the PMATAC clusters elongate along the tensile direction, generating anisotropic ionic-bond-rich domains. B Orientation evolution of PAAc and PMATAC chains during stretching. PAAc chains orient nearly linearly with strain, while PMATAC remains isotropic until \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ > 3, when weak alignment emerges (Herman’s factor <0.2). C Variation of normalized atomic number density in PMATAC-rich region (corresponding to the ionic-bond-rich region) and PAAc-rich region (corresponding to the hydrogen-bond-rich region). At small strains, both densities decrease slightly and remain comparable; at larger strains, they diverge, and the PAAc-rich region becomes less dense, matching the onset of macroscopic whitening. The mechanism of stretch-induced whitening and crack resistance. A All-atom molecular dynamics (MD) simulations reveal the evolution of microscopic structure during stretching, consistent with scattering observations. Among them, the PMATAC cluster was yellow, the PAAc cluster was blue, and the water molecules were gray. At \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 1, dispersed PMATAC clusters are embedded in the anionic matrix; at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 3, deformation of the anionic chains and lateral contraction compress the less-deformable cationic clusters, driving them to aggregate and form laterally aligned heterostructures (red dashed region); at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 6, the PMATAC clusters elongate along the tensile direction, generating anisotropic ionic-bond-rich domains. B Orientation evolution of PAAc and PMATAC chains during stretching. PAAc chains orient nearly linearly with strain, while PMATAC remains isotropic until \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ > 3, when weak alignment emerges (Herman’s factor <0.2). C Variation of normalized atomic number density in PMATAC-rich region (corresponding to the ionic-bond-rich region) and PAAc-rich region (corresponding to the hydrogen-bond-rich region). At small strains, both densities decrease slightly and remain comparable; at larger strains, they diverge, and the PAAc-rich region becomes less dense, matching the onset of macroscopic whitening. Analysis of individual chain trajectories (Supplementary Fig. 15) highlights a sequential deformation process: the PAAc chains undergo early straightening and orientation, whereas the polycationic chains engage only at higher strains and remain partially unextended. To clarify the global structural evolution, we extracted Herman’s Orientational Factor (HOF) from the trajectories. Figure 4B shows the orientation of the cationic and anionic chains: in the initial stage (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ < 3), the PAAc chains increase almost linearly in orientation, whereas the PMATAC chains show little change. This indicates that PAAc deforms first while the cationic clusters deform only slightly, and further suggests that dynamic hydrogen-bond dissociation/association and chain disentanglement among PAAc are the main contributors to the initial modulus and the yielding plateau. When \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ > 3, the PMATAC chains begin to develop weak orientation (HOF < 0.2), while the PAAc orientation continues to rise, reaching a HOF of ~0.65. Two equal-volume subregions in the undeformed model were defined, with one PMATAC-rich (corresponding to the ionic-bond-rich) region and the other PAAc-rich (corresponding to the hydrogen-bond-rich) region. During tensile deformation, the normalized atomic number density in the PAAc-rich region steadily decreases. At low strain levels, both domains show only a slight reduction in density and remain nearly identical; however, with increasing strain, their densities diverge, and the PAAc-rich domain becomes markedly less dense than the PMATAC-rich domain (Fig. 4C). This growing density contrast corresponds directly to the macroscopically observed whitening. Fracture toughness and crack resistance of the hydrogel The single-notch tests were used primarily to visualize the nucleation and growth of the crack-tip whitening zone, as well as the associated crack blunting behavior during stretching. For the 1:2.5 non-whitening gel, a 1 mm notch triggers rapid crack propagation and catastrophic failure at a stretch-rate of 100 mm min-1 (Fig. 5A and Supplementary Movie 2). By contrast, the 1:3.5 whitening gel exhibits dynamic crack blunting (Fig. 5B). By \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 3.5 (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\varepsilon$$\end{document}ε = 250%), a whitening zone is already evident around the crack tip, indicating that localized energy dissipation has begun. With further stretching, the zone enlarges and becomes opaquer, effectively shielding the tip. At \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda=$$\end{document}λ= 9, whitening pervades the entire specimen, and the initially sharp notch transforms into a blunted, straight profile. This evolutionary process implies that locally high-strain crack tips are frozen, and the concentrated stresses at the tip are effectively transferred and dispersed to other regions, gradually forming an extensive fracture process zone. The energy required for crack propagation is dissipated by forming new interfaces behind the blunted tip, rather than concentrating at a single failure point. This intrinsic damage tolerance thus derives from a local mechanical-feedback mechanism: high strain concentration at the crack tip triggers strain-induced macroscopic phase separation precisely where it is needed, blunting the tip, redistributing stress over a wider region, and erecting a robust whitening barrier against further propagation.Fig. 5Strain-adaptive crack suppression and tunable fracture toughness.A Representative 1:2.5 non-whitening gel: a 1 mm notch causes rapid crack propagation and early failure. B Representative 1:3.5 whitening gel: a whitening zone nucleates near the notch (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 3.5), grows with strain, and blunts the crack; by \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 9 the notch becomes a straight, blunted profile, evidencing an extensive process zone and strong crack shielding. C Fracture toughness measured from pure-shear tests: whitening gels exhibit toughness\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\,\approx \,$$\end{document}≈35–70 kJ m−2, over an order of magnitude higher than non-whitening ones. Bars represent mean values, error bars represent s.d., and dots represent individual measurements. D Strain-rate dependence: toughness increases sharply once whitening occurs above \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\approx$$\end{document}≈10 mm min−1, reaching a maximum of \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\approx$$\end{document}≈100 kJ m−2. E Temperature dependence of fracture toughness: toughness decreases with temperature and collapses above\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\,\approx$$\end{document}≈50 °C as whitening disappears. F A notch is introduced during the stretching process. The 1:2.5 non-whitening hydrogel rapidly fractures after a cut is introduced at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda \approx \,$$\end{document}λ≈4–4.5. G The 1:3.5 tensile-whitening hydrogel shows immediate whitening around the notch at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 5, which expands with increasing strain to \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 7 while the crack length remains nearly unchanged. H Schematic of the crack resistance from combined scattering, simulation and DIC results: strain-induced macroscopic phase separation and anisotropic alignment of ionic-bond-rich domains expand the fracture process zone and enable efficient stress redistribution. Data are presented as mean ± s.d. (n ≥ 3). Scale bars are 5 mm. Strain-adaptive crack suppression and tunable fracture toughness. A Representative 1:2.5 non-whitening gel: a 1 mm notch causes rapid crack propagation and early failure. B Representative 1:3.5 whitening gel: a whitening zone nucleates near the notch (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 3.5), grows with strain, and blunts the crack; by \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 9 the notch becomes a straight, blunted profile, evidencing an extensive process zone and strong crack shielding. C Fracture toughness measured from pure-shear tests: whitening gels exhibit toughness\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\,\approx \,$$\end{document}≈35–70 kJ m−2, over an order of magnitude higher than non-whitening ones. Bars represent mean values, error bars represent s.d., and dots represent individual measurements. D Strain-rate dependence: toughness increases sharply once whitening occurs above \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\approx$$\end{document}≈10 mm min−1, reaching a maximum of \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\approx$$\end{document}≈100 kJ m−2. E Temperature dependence of fracture toughness: toughness decreases with temperature and collapses above\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\,\approx$$\end{document}≈50 °C as whitening disappears. F A notch is introduced during the stretching process. The 1:2.5 non-whitening hydrogel rapidly fractures after a cut is introduced at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda \approx \,$$\end{document}λ≈4–4.5. G The 1:3.5 tensile-whitening hydrogel shows immediate whitening around the notch at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 5, which expands with increasing strain to \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 7 while the crack length remains nearly unchanged. H Schematic of the crack resistance from combined scattering, simulation and DIC results: strain-induced macroscopic phase separation and anisotropic alignment of ionic-bond-rich domains expand the fracture process zone and enable efficient stress redistribution. Data are presented as mean ± s.d. (n ≥ 3). Scale bars are 5 mm. Fracture toughness under different conditions was quantified using the pure-shear tests51,52. Specifically, the stretch at crack initiation (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\lambda }_{C}$$\end{document}λC) in the precut specimen was recorded, and the strain energy density was obtained by integrating the stress-strain curve of the corresponding uncut specimen to the same stretch, from which \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${G}_{c}$$\end{document}Gc was calculated (see Methods and Supplementary Fig. 16)53,54. The results show that, for the non-whitening gel (Supplementary Fig. 17A), once a crack initiated, it propagated rapidly to failure-the inset reveals the crack swiftly traversing the specimen, indicating brittle fracture. By contrast, in the tensile-whitening gel (Supplementary Fig. 17B), a pronounced whitening band developed at the crack tip with increasing strain, which effectively suppressed further crack advance. Across compositions, the whitening gels exhibited fracture toughness exceeding that of the non-whitening gels by over an order of magnitude, rising from 2 to 3 kJ m-2 to ≈ 35–70 kJ m−2 (Fig. 5C). This confirms that strain-induced macroscopic phase separation and microstructural reorganization are the key to enhanced toughness. The dynamic physical crosslinks make fracture toughness highly tunable, enabling the network to adapt its dissipation capacity to the loading environment. Figure 5D shows that toughness strongly depends on strain rate: at low rates (leftmost points), the gel remains transparent with toughness <10 kJ m-2; at rates above ≈10 mm min−1, tensile whitening emerges and toughness rapidly rises, reaching ≈100 kJ m−2 (Supplementary Fig. 18). This indicates that the formation of dissipative structures at the crack tip is rate-controlled, with energy dissipation primarily originating from viscoelastic losses in the phase-separated domains and interfacial dissipation. Figure 5E shows that the fracture toughness decreases monotonically with increasing temperature and drops sharply to ≈4 kJ m−2 above 50 °C, where whitening disappears (Supplementary Fig. 19). This suggests that the whitening-assisted toughening mechanism has a thermal stability limit: at elevated temperature, faster relaxation of dynamic ionic and hydrogen-bonded interactions reduces the density contrast and structural persistence of the phase-separated domains, so that the crack-tip dissipative structure can no longer be maintained. Notably, the fracture toughness of the transparent gel remains competitive among hydrogels11,31,32. In high-stress engineering scenarios, hydrogels inevitably come into contact with rigid materials. Sharp edges can introduce surface cuts during stretching, often leading to catastrophic failure. Here, we demonstrate the exceptional crack-growth resistance of the tensile-whitening hydrogel under such extreme conditions. During the continuous stretching (at a speed of 100 mm/min), a sharp blade was used to introduce a notch corresponding to ~40% of the sample width. As shown in Fig. 5F, the tensile non-whitening gel fractured immediately after the cut, whereas the whitening gel exhibited a distinct whitening zone nucleating around the notch at \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 5 (Fig. 5G). With further stretching to \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 7, the whitening zone gradually shrank to a triangular region with its apex at the crack tip. This dynamic evolution visualizes the stress-release pathway of a soft, physically crosslinked material under coupled large deformation and fracture, offering a direct and intuitive experimental route to probe stress redistribution in soft networks under complex loading. The strain field evolution at the crack tip was captured in situ using a digital image correlation (DIC) system to visualize deformation during uniaxial stretching of notched samples (Supplementary Fig. 20). For the tensile-whitening hydrogel, when the local strain at the crack tip reaches \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda$$\end{document}λ = 5, the strain-growth rate near the tip gradually decreases, while regions farther away from the crack tip begin to deform rapidly. Eventually, most of the gel reaches a nearly uniform strain distribution. Based on the combined experimental and simulation results, we propose a mechanistic model for the crack-propagation resistance of tensile-whitening hydrogels (Fig. 5H). During stretching, the region immediately ahead the crack tip undergoes the highest strain rate, leading to rapid local deformation. Once the local hardening strain is reached, macroscopic phase separation and alignment of ionic-bond-rich domains first emerge at the crack tip, serving as dissipative barriers to hinder crack advancement. Owing to the interpenetrated molecular connectivity between the two phases (with no discrete interface) and the dynamically dissociable and deformable ionic-bond-rich hard phase, the hydrogel network exhibits an exceptionally efficient stress-transfer capability30,36. Consequently, the high stress at the crack tip is rapidly redistributed throughout the network, allowing strain in distant regions to increase gradually; as a result, the fracture process zone (FPZ) expands rapidly. Ultimately, the entire hydrogel reaches a uniform strain state and undergoes global rupture, rather than catastrophic crack propagation. Discussion The work designs a mechanically adaptive tough hydrogel that reconciles high stiffness, large extensibility, and exceptional crack resistance within a structurally simple, physically crosslinked network. In contrast to many state-of-the-art tough and crack-resistant hydrogels11,18–23,31–33,55, our system starts from an isotropic, optically transparent polyelectrolyte complex and develops anisotropic dissipation pathways only when and where large deformation is imposed. The asymmetric pairing of a strong cationic and a weak anionic polyelectrolyte breaks the conventional requirement for strict charge stoichiometry in PIC hydrogels, driving the formation of ionic-bond-rich and hydrogen-bond-rich domains that are initially difficult to distinguish at the mesoscale. Under load, however, this latent compositional asymmetry is converted into a pronounced mechanical asymmetry. Hydrogen bond-rich regions deform and relax rapidly, while ionic bond-rich domains resist deformation and eventually align along the tensile direction, producing a strain-induced macroscopic phase separation that both governs energy dissipation. This mechanochemical transduction mechanism complements and extends existing design frameworks for tough hydrogels, in which energy dissipation is commonly built into the initial microstructure rather than that dynamically generated by the mechanical field11,31–33. Our multiscale characterization also clarifies how the present whitening mechanism differs from several established toughening routes in hydrogels. First, it differs from lower-hydration, densification-dominated systems, where reinforcement is commonly associated with reduced water content, chain packing, and entanglement9,10,24. In our system, however, the in-situ WAXS response is similar in the whitening and non-whitening gels, with both showing reduced interchain spacing and enhanced chain alignment under strain, indicating that molecular-scale densification alone is not sufficient to explain the pronounced difference in crack resistance. Instead, the mesoscale amplification of density contrast and the anisotropic reorganization of ionic-bond-rich domains are directly correlated with macroscopic whitening and crack-tip protection. Second, it differs from crystallization-based PVA systems. Extensive and elegant studies by Zhao et al. have demonstrated strong fatigue resistance in low-hydration PVA hydrogels, where reinforcement is typically associated with crystallite/nanofibril formation or pre-engineered anisotropic hierarchical architectures13,14. By contrast, the present hydrogel starts from a macroscopically transparent and isotropic network and develops crack-tip protection adaptively only under load. Third, it also differs from previously reported bicontinuous, microphase-separated, and double-network hydrogels. In those systems, the key dissipative pathways are largely predefined during fabrication, or fracture energy is mainly supplied by irreversible scission of a brittle network22,23,56. For example, bicontinuous self-healing hydrogels enhance fatigue resistance by distributing energy across percolated soft and hard pathways16,38,39, but their microstructure is largely set during fabrication and only evolves modestly under load. In the present system, the ion-rich domains instead serve as reconfigurable hard phases, which stiffen at high strain, act as crack arrestors, and still recover via reversible ionic dissociation and reassociation. This dynamic compositional asymmetry and hierarchical structural reorganization cooperate to transform localized stress concentration into spatially distributed deformation and, ultimately, global rupture without catastrophic crack propagation16,29,33,43,44. We have developed a general strategy for creating adaptive, damage-tolerant hydrogels with a strain-activated macroscopic phase separation between two dynamically bonded phases. The asymmetric polyelectrolyte complexation platform offers a broad design space, such as charge ratio and ionization degree of the weak polyelectrolyte. In the meanwhile, the temperature or loading rate jointly control the mechanical performance. Accordingly, the whitening-assisted toughening effect is most pronounced below 50 °C and at strain rates above 1.6 \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\times$$\end{document}×10−2 s−1. The high modulus and ultrahigh fracture toughness achieved in this work, together with the visual readout of damage through reversible whitening, make these hydrogels promising candidates for load-bearing biointerfaces, damage-tolerant soft robotic components operating under extreme or intermittent mechanical loading, and protective coatings where early warning and suppression of crack growth are critical. In addition, integrating this mechanically triggered whitening/phase-amplification mechanism with other noncovalent motifs or with spatial patterning may enable soft materials that not only withstand complex mechanical histories but also encode, visualize, and actively regulate them, further narrowing the gap between synthetic hydrogels and the adaptively tough architectures that exist in biological tissues34,36. Methods Materials preparation Acrylic acid (AAc), Methacrylatoethyl trimethyl ammonium chloride (MATAC), 2-Ketoglutaric acid (photoinitiator) were purchased from Sigma-Aldrich. Millipore deionized water (resistivity: 18.2 MΩ/cm) was used in all experiments. The cationic monomer was photopolymerized in water at a concentration of 2 M using α-ketoglutaric acid as the initiator. Then, the product was dried to remove moisture and was prepared for use. A specific amount of solid PMATAC was weighed. A predetermined proportion of AAc and a photoinitiator (0.5% of the total monomer molar quantity) were added, followed by the addition of deionized water to achieve a total monomer molar concentration of 3 M. In this work, reported compositions such as 1:3 and 1:3.5 refer to the monomer feed molar ratio of MATAC to AAc in the precursor formulation. Unless otherwise specified, all formulations discussed in this manuscript are denoted by this feed-ratio notation. The mixture was stirred thoroughly until all solid components were dissolved. The resulting homogeneous solution was purged with argon gas for 10 min to remove dissolved oxygen and subsequently transferred into a glass mold. Finally, the solution in the mold was exposed to double-sided ultraviolet irradiation at a wavelength of 365 nm and polymerized at room temperature for 8 h to initiate free radical polymerization. The as-prepared PAAc/PMATAC hydrogel was immersed in a large amount of deionized water, and the water was changed every 12 h. The gels reached an equilibrium state after 5 days of immersion. Mechanical tests The mechanical properties of the hydrogels were tested on a commercial tensile tester (Instron 3343). The hydrogel sheets were cut into dumbbell-shaped samples with an initial gauge length of 12 mm and a width of 2 mm. Uniaxial tensile tests were performed on the samples at a specific stretching rate at a specific temperature. The nominal stress and engineering strain were recorded, and Young’s modulus was extracted from the initial slope of the tensile stress–strain curve with an engineering strain below 20%. Throughout this manuscript, the stretch ratio is defined as \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda=L/{L}_{0}$$\end{document}λ=L/L0, and the corresponding engineering strain is \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\,\varepsilon=(\lambda -1)\times 100\%$$\end{document}ε=(λ−1)×100%. Young’s modulus, tensile strength, elongation at break, and fracture energy are reported as mean ± s.d. from n = 5 independent tensile specimens. Representative stress–strain curves are shown where indicated, while the corresponding summary plots are based on the averaged values. For pure shear tests, hydrogels with identical dimensions (a width of 50 mm, a height of 10 mm, and a thickness of about 0.7 mm) were employed. Several samples were precut with a 15 mm-long crack before testing. For each fracture-toughness measurement, the uncut and precut samples were tested under the same loading condition, including the same strain rate and water-bath temperature. The fracture stretches of uncut/precut samples were labeled as \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\lambda }_{{f}}$$\end{document}λf and \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\lambda }_{c}$$\end{document}λc, respectively. The area underneath the nominal stress–stretch ratio curve of the uncut sample gives the strain energy density \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$W(\lambda )$$\end{document}W(λ). The fracture toughness was calculated as \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${G}_{c}=W({\lambda }_{c})\times H$$\end{document}Gc=W(λc)×H, where \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${H}$$\end{document}H is the reference height of the sample and was fixed at 10 mm for all pure-shear tests49,50. Fracture toughness is reported as mean ± s.d. from n = 3 independent pure-shear tests. Rheological behaviors of the as-prepared hydrogels were investigated via small-amplitude oscillatory shear using a DHR-2 rheometer (TA Instruments). Two parallel plates with different diameters (8 or 25 mm) were chosen according to the stiffness of the samples. Disk-shaped hydrogels with a thickness of 1 mm were placed between the parallel plate and the rheometer. An appropriate axial force (0.1–5 N, depending on the stiffness of samples) was applied during the rheological measurements. The edge of the gel sample was sealed with liquid wax to prevent water evaporation during the measurement. An advanced strain sweep at a frequency of 10 rad/s was applied on each sample to ensure the applied strain amplitude in the linear viscoelastic region. The temperature scan was performed on the hydrogel, with a heating rate of 3 °C/min. Characterizations The interactions between ionic bonds and hydrogen bonds during the swelling process of this hydrogel were characterized by attenuated total reflectance Fourier transform infrared spectroscopy (Nicolet iS10 ATR-FTIR; Thermo Scientific). The spectra were obtained with 32 scans and 4 cm−1 resolution in the range 4000–400 cm−1. The transmittance of the gel was recorded by a UV–vis spectrophotometer (Shimadzu, UV-2550) at a wavelength of 500 nm. Atomic force microscopy in combination with infrared spectroscopy (AFM–IR) was conducted by a multimode AFM microscope (Nano-IR2-FS, Anasys Instruments) with the contact mode at a fixed wavenumber of 1710 cm−1, highlighting the distribution of carbonyl groups. SAXS and WAXS measurements of the gel were carried out at the BL16B1 beamline of the Shanghai Synchrotron Radiation Facility of China (SSRF). The wavelength of the X-ray was 1.24 Å, and the sample-to-detector distance was 2091 mm. USAXS measurements of the gel were performed at the BL10U1 beamline of the SSRF. The wavelength of the X-ray was 1.24 Å, and the sample-to-detector distance was 28,922 mm. The two-dimensional (2D) scattering patterns were collected by a Pilatus 2 M detector with a resolution of 1475 × 1679 pixels and a pixel size of 172 × 172 μm2. Multiple square hydrogel slices were cut at different swelling stages and immediately used for measurement, with an exposure time of 10 s during measurement. To minimize the influence of solvent evaporation, polyimide films were attached to both sides of the gel. Fit 2D software was used to deduct background scattering signal and extract one-dimensional (1D) USAXS and SAXS profiles by circularly integrating the 2D patterns. The 1D profiles were fitted with a model using SasView-5.0.5. The Gel-Fit model expression is as follows44,48:1\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\,I\left(q\right)\approx \frac{{I}_{L}\left(0\right)}{{\left(1+\left[\frac{D+1}{3}\right]{q}^{2}{\xi }^{2}\right)}^{\frac{D}{2}}}+{I}_{G}\left(0\right)\cdot \exp \left(-\frac{{q}^{2}{R}_{g}^{2}}{3}\right)+B$$\end{document}Iq≈IL01+D+13q2ξ2D2+IG0⋅exp−q2Rg23+Bwhere IL(0) represents the initial scattering intensity of the Lorentz component, D denotes the fractal dimension (typically between 2 and 4), and \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\xi$$\end{document}ξ characterizes the rapid fluctuations in polymer chain positions, serving here as the variable periodic distance between the two enriched phases47,48. IG (0) denotes the initial scattering intensity of the Guinier component, and Rg represents the static stacking volume of polymers fixed by polymer clusters or such aggregates47-i.e., the size of the enriched phase. B indicates the background of the integral curve. Molecular dynamics simulation The initial atomic model of the asymmetric polyelectrolyte hydrogel was constructed to replicate the experimental system, comprising 30 chains of polycation PMATAC (degree of polymerization, DP = 40) and 60 chains of polyanion PAAc (DP = 60) at a deliberate 1:3 molar ratio within a cubic simulation box with initial dimensions of approximately 250 × 250 × 250 Å3. The initial amorphous configuration was generated using PACKMOL, which was subsequently solvated with 12,000 water molecules using the SPC/E model. Chloride counterions were added to ensure charge neutrality of the overall system. All interatomic interactions were described by the OPLS-AA force field. Long-range electrostatic interactions were resolved using the Particle-Particle Particle-Mesh (PPPM) solver with a precision of 10−4, while short-range van der Waals interactions were truncated at a cutoff distance of 12 Å. Periodic boundary conditions were applied in all three directions, and the SHAKE algorithm was applied to constrain high-frequency bond vibrations involving hydrogen atoms. All molecular dynamics simulations were performed using the Large-scale Atomic/Molecular Massively Parallel Simulator (LAMMPS) package, and visualization of the simulation trajectories was performed using the Open Visualization Tool (OVITO). The simulation workflow initiated with energy minimization using the conjugate gradient algorithm to relieve any local steric clashes. The equations of motion were integrated using the Velocity-Verlet algorithm with a time step of 1.0 fs. The system was then equilibrated under isothermal-isobaric (NPT) conditions at 1 atm through a two-stage protocol. Namely, it was first heated from 100 K to the target temperature of 300 K over 0.5 ns, followed by an extensive 20 ns relaxation period at 300 K, maintained using the Nosé-Hoover thermostat and barostat. For mechanical characterization, uniaxial tensile deformation was applied along the Z-axis at a constant engineering strain rate of 5 × 10⁸ s⁻¹. During deformation, the transverse dimensions (X and Y) were independently coupled to the barostat to maintain zero lateral stress (1 atm), allowing for natural Poisson contraction. The atomic stress tensor was computed at regular intervals using the virial theorem. To quantitatively correlate with scattering data, the chain orientation degree of both polyelectrolytes during stretching was characterized by calculating Herman’s orientation factor for the polymer backbones relative to the tensile direction. Furthermore, to decipher the mechanism behind the macroscopic whitening, the simulation box was partitioned into 27 sub-regions. The sub-region with the highest concentration of cationic (PMATAC) chains was defined as the ionic-bond-rich domain, while the one with the highest concentration of anionic (PAAc) chains was defined as the hydrogen-bond-rich domain. The temporal evolution of the respective polyion densities in these two representative domains was tracked throughout the tensile deformation to monitor the strain-induced density divergence process. Supplementary information Supplementary Information Description of Additional Supplementary Files Supplementary Movie 1 Supplementary Movie 2 Supplementary Movie 3 Supplementary Data 1 Transparent Peer Review file Supplementary Information Description of Additional Supplementary Files Supplementary Movie 1 Supplementary Movie 2 Supplementary Movie 3 Supplementary Data 1 Transparent Peer Review file Source data Source Data Source Data