Synthesis, characterisation and electrochemical behaviour of calcium carbonate nanoparticles derived from automobile oxy-acetylene gas welding waste Authors: Nnabuk Okon Eddy, Sunday Nweze, Ifeanyi Samson Eze, Rajni Garg, Raymond Taziwa, Hamimullah Watandost Published: 2026 ABSTRACT In actualizing the management of this toxic waste, resource recovery was designed to convert the Ca(OH)2 rich waste (generated by automobile welding process) to calcium carbonate nanoparticles (CaCO3NPs). The synthesized nanoparticles were characterized using XRF, SEM–EDX, XRD, FTIR, XPS, TGA/DTA, BET, DFT and EIS. Results from XRF and SEM–EDX analyses showed calcium as the dominant element, with CaO and Ca contents of 98.59 wt% and 84.30 wt%, respectively. However, based on XRD, XPS, XRF and SEM–EDX results, minor impurities, including Si Al, Fe, and Mg, were also detected at concentrations less than 0.2% respectively.. SEM micrographs also showed rough, irregular, partially agglomerated surfaces and features that reflect heterogeneous particle sizes. XRD patterns identified a dominant calcite phase (~ 81%) and minor vaterite (< 19%), with crystallite sizes ranging from 12.0 to 21.6 nm (average 16.28 nm) while the FTIR spectrum showed characteristic carbonate vibrations at 1507.71, 1149.88, and 877.79 cm⁻1, that futher confirms high purity. Thermal analysis of the nanoparticles indicated initial weight loss of less than 3% below 200 °C due to adsorbed moisture, and complete decomposition between 600 and 850 °C, with an activation energy of 178 kJ/mol and estimated purity of 97.75%. BET and DFT analyses revealed high surface areas (134 m2/g, BET; 36.6 m2/g, DFT), mesoporous structure, average pore diameter of 2.65 nm, pore volume of 0.16678 m3/g, and surface area-to-volume ratio of 819 m⁻1. Electrochemical impedance spectroscopy in 0.5 M H2SO4 showed two relaxation processes in Nyquist plots. The first relaxation represented a high-frequency grain boundary processes having Rct = 4.0 × 10⁶ Ω, C = 3.98 × 10⁻⁹ F, τ = 0.016 s, θmin = 43°, n = 0.38, Q = 1.66 × 10⁻⁸ S sn, and Cdl = 204 μF, indicating dispersive capacitive behaviour and significant interfacial polarization. However, the low-frequency bulk charge transfer processes had Rct = 2.4 × 10⁷ Ω, C = 2.10 × 10⁻13 F, τ = 5.03 × 10⁻⁶ s, θmin = 73°, n = 0.81, Q = 1.36 × 10⁻12 S sn, and Cdl = 34.3 μF, indicating high resistance and dielectric behaviour. Frequency-dependent capacitance analysis further confirmed strong double-layer formation at low frequencies and intrinsic insulating characteristics at high frequencies. The combination of nanoscale dimensions, high surface area, mesoporosity, thermal stability, wide bandgap (6.01 eV), and distinctive electrochemical behaviour indicated that the CaCO3NPs has potentials for dielectric fillers, corrosion-resistant coatings, adsorbents, and inert supports in electrochemical applications. Introduction Several nations are faced with challenges associated with waste management regarding cost, best disposal options, environmental and other barriers. Among numerous options that have been practised over the years, resource recovery, reuse and recycling have proven to be the best options, because they have the capacity to provide multiple solutions to environmental and industrial challenges, cost reduction and reductions in the volume of wastes [49]. Automobile welding utilizes acetylene gas generated by the reaction of calcium carbide and water for welding metallic components as shown in Eq. 1.1\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$ {\mathrm{CaC}}_{2} + {\mathrm{H}}_{2} {\mathrm{O}} \to {\mathrm{C}}_{2} {\mathrm{H}}_{2} + {\mathrm{Ca}}\left( {{\mathrm{OH}}} \right)_{2} $$\end{document} The acetylene gas has properties that favour its application in welding metallic components of automobiles through the generation of a high temperature, localized flame, rapid combustion/energy release, controllability, reducing properties and compatibility with various metals [66, 74]. The consequence of Eq. 1 is that calcium hydroxide, which is a by-product of the process, is normally discarded into the surrounding environment without immediate usage. The generated calcium hydroxide-rich waste can negatively impact the soil and water, either directly or through interaction with other contaminants in the environment [1]. Although some beneficial roles of low Ca(OH)2 have been reported, such as the maintenance of soil pH, promotion of soil aggregation and nutrient availability [67]. There are supporting literature that have shown that at moderate concentration, the presence of Ca(OH)2 can lead to several environmental challenges including the suppresion of microbial activity in the soil, acceleration of the deficiency of essential elements (such as Fe, P, Mn, etc.), obstruction of soil aeration, reduction in the rate of nitrification and enhancement of the degradation of soil structure and associated consequences [81]. Also, consequences of deliberate application of \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\mathrm{C}\mathrm{a}(\mathrm{O}\mathrm{H})}_{2}$$\end{document} for the adjustment of soil or water pH ca lead to severe and harmful impacts on aquatic life, enhance light penetration, corrosion and scaling of pipelines, boilers and industrial installations [41, 50, 51, 57, 76]. Furthermore, this by-product can also be enriched with other contaminants (such as heavy metals), when disposed to the environment, thereby enhancing their toxicity. In consideration of the listed and other negative impacts of \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\mathrm{C}\mathrm{a}(\mathrm{O}\mathrm{H})}_{2}$$\end{document} on the environment, calcium hydroxide is classified as hazardous waste [69]. Consequently, its disposal to the environment is under regulation [75]. Unfortunately, most artisans in automobile workshops have violated existing regulations because some of them lack adequate environmental education, while others may not be willing to bear the disposal or treatment cost. The prevailing disposal option among automobile welders (i.e. direct discharge to the environment), renders the product to be susceptible to further reactions and further accerelation of toxicity life cycle. Resource recovery, recycling or reuse can solve the challenges that are associated with the disposal of this hazardous waste [63]. Some avenues concerning the application of \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\mathrm{C}\mathrm{a}(\mathrm{O}\mathrm{H})}_{2}$$\end{document} from automobile welding waste have been reported, but with additional consequences as lsted earlier. However, none have been reported on the conversion of \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\mathrm{C}\mathrm{a}(\mathrm{O}\mathrm{H})}_{2}$$\end{document} to calcium carbonate nanoparticles, nor on the investigation of its potential for application in electrochemical systems. Based on available literature, the applications of \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\mathrm{C}\mathrm{a}\mathrm{C}\mathrm{O}}_{3}\mathrm{N}\mathrm{P}s$$\end{document} have a broader industrial scope especially in biomedical (drug delivery, bone tissue engineering, contrast agent), environmental (water treatment and carbon (IV) oxide sequestration), agriculture (soil pH adjustment and pest control), food industries (as food additive and nutraceuticals), cosmetic and personal care (cosmetic formulation and antimicrobial applications), material science (in formulation of nanocomposites and applications in paint and coating), pharmaceutical (as excipient in tablet and the formulation of antacid) and in the chemical industries as a pH regulator [18, 42, 52, 78, 85]. The major advantages and current application routes of CaCO3 nanoparticles may be promoted by their relatively low toxicity [11], relative stability, biocompatibility and biodegradability [85], pH-responsive behaviour [39], surface functionality capacity [44], crystalline polymorphism [21] and unique mechanical properties [47]. Consequently, applications in the energy sector will depend on its electrochemical behaviour, especially when considering capacitance, impedance, resistance, double layer and some interfacial properties [27, 45, 54]. The choice of calcium carbonate nanoparticles (CaCO3NPs) in this study is based on the need to take advantage of resource revovery from automobile welding waste, the stability of CaCO3NPs and the promotion of sustainable conversion of hazardous automobile welding waste into a value-added material. CaCO3NPs possess advantageous properties such as low toxicity, high surface area, polymorphism and pH-responsive behaviour. These properties can enhance them to be suitable for diverse industrial and electrochemical applications at low cost. At present, the literature is scanty regarding the electrochemical application of calcium carbonate nanoparticles, except, the reported investigation by Ramasamy et al. [61] on the potential of PEG/CaCO3 nanoparticles as an effective capacitor. Therefore, the investigation of the management of automobile welding waste and consequence search for their potential in electrochemical system have significant scientific benefits, especially, if achieved at a level that support sufficient availability of economical, eco-friendly and accessible raw materials for its synthesis. Ongoing processes have employed several synthetic routes for the production of CaCO3NPs, including green synthesis, homogenization method, chemical reaction method, precipitation, slow carbonation and polymer-mediated method [2, 19, 25, 64]. Most of these methods have been commended to a good extent based on the quality of the product. However, some of the reported challenges include non availability of commercial quantity of raw materials at low cost, low product yield, expensive technology, low quality product, etc. [85]. In addition, the methods may be selective and inapplicable to some potential precursors. Consequently, method development or modification for the synthesis and application of CaCO3NPs from automobile welding waste may provide additional support and solutions for solving some of the listed challenges. This will also provide an avenue for effective management of the automobile waste byproduct. In this work, we report for the first time a method modification for the synthesis, characterization and electrochemical investigation of \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\mathrm{C}\mathrm{a}\mathrm{C}\mathrm{O}}_{3}\mathrm{N}\mathrm{P}s$$\end{document} from automobile acetylene welding waste. To the best of our knowledge, this specific waste stream has not been reported before. The employment of automobile waste for the production of \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\mathrm{C}\mathrm{a}\mathrm{C}\mathrm{O}}_{3}\mathrm{N}\mathrm{P}s$$\end{document} has some advantages over most sources, such as biogenic (egg and crustacean shells), because resources are recovered from a toxic source, unlike biogenic and other materials. Consequently, a dual solution is envisaged, including hazardous waste management through a waste-to-resource approach and the production of useful nanoparticles. Also, unlike previous studies, which largely considered adsorption and structural variables, the present work extends the investigation to electrochemical characterisation. Materials and methods Materials The major materials that were useful for the study were Na2CO3 and waste materials containing Ca(OH)2 (obtained from some automobile welding workshop in Mechanical village, Apo, Abuja in Nigeria. The waste samples were obtained directly from the discharge tank to avoid contamination if disposed to the environment. The sample was dried under the sun and in the oven for further removal of moisture. The prepared sample was stored in a dissicator. Methods 10 g of the Ca(OH)2 rich waste was concentrated in deionized water to obtained uniform Ca(OH)2 suspension. 2.65 g of anhydrous sodium carbonate were dissolved in 250 mL of deionized water to obtain a 0.1 M Na2CO3 solution. The Na2CO3 solution was reacted with the Ca(OH)2 suspension in a beaker and continuously stirred at room temperature to enhance dissolution and fasten the reaction rate to completion. The observed reaction produced calcium carbonate precipitate according to the following equation\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\mathrm{C}\mathrm{a}\left(\mathrm{O}\mathrm{H}\right)}_{2}+ {\mathrm{N}\mathrm{a}}_{2}{\mathrm{C}\mathrm{O}}_{3} \to 2\mathrm{N}\mathrm{a}\mathrm{O}\mathrm{H}+ {\mathrm{C}\mathrm{a}\mathrm{C}\mathrm{O}}_{3}$$\end{document} The precipitated \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${CaCO}_{3}$$\end{document} particles were separated from the NaOH by vacuum filtration and were washed to ensure that all the NaOH (which is soluble in water) were removed. After precipitation, the products were subjected to vaccum filtration and extensively washed several times with deionized water, seeing that NaOH is highly soluble in water, repeated washing ensured effective removal of NaOH. Therefore, the washing process as reported in the manuscript serves as the (ii) Thermal treatment (calcination control). The completeness of washing was confirmed by testing the filtrate with pH paper and phenolphthalein indicator. The absence of a pink colouration and a neutral pH indicated that residual hydroxides had been effectively removed. After washing, the filtrates were dried in an oven set to 80 °C for 4 h. The dried calcium carbonate was finally calcinated at 650 °C to convert it to \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\mathrm{C}\mathrm{a}\mathrm{C}\mathrm{O}}_{3}\mathrm{N}\mathrm{P}s$$\end{document} and to removed any residual or other unwater adsorbed materials. The calcination temperature of 650 °C was selected based on pretrial experiments, which showed that close to this temperature, the materials undergo conversion to nanoparticles. This temperature is sufficient to induce controlled thermal activation without complete structural collapse of the nanoparticles. The synthesis route adopted in this study is inherently scalable, as it involves simple precipitation and filtration steps that can be readily translated to large-scale continuous or batch processing systems. The use of readily available Ca(OH)2-rich waste as a precursor further supports scalability by ensuring a consistent and low-cost raw material supply. Characterization The following characterisation techniques were employed to ascertain the product composition and other functional characteristics, namely, UV–visible, Fourier transformed infrared (FTIR, X-ray diffraction (XRD), X-ray fluorescence (XRF), SEM–EDX, XPS, TGA/DTA and BET. UV–visible spectroscopy The analysis of the optical properties of the CaCO3 nanoparticles was carried out using Shimadzu UV-1800 UV–Visible Spectrophotometer. About 10 mg of the dried CaCO3 nanoparticles was dispersed in 100 mL of deionized water to obtain a concentration of 0.1 mg/mL. The suspension was ultrasonicated for 20 min to ensure uniform dispersion. Approximatly, 3 mL of the dispersion was transferred into a quartz cuvette using a 1 cm path length. The absorbance spectrum was recorded over the wavelength range of 200–800 nm at room temperature, using deionized water as the blank reference. The recorded values were used to plot a graph of absorbance against wavelength in order to evaluate the maximum wavelength of absorption and the band gap. X-ray diffraction (XRD) analysis The crystalline structure, phase composition, and crystallite nature of the synthesized CaCO3 nanoparticles were investigated using an Rigaku SmartLab X-ray Diffractometer operated with Cu Kα radiation (λ = 1.5406 Å), manufactured by Rigaku. About 1.0 g of the finely powdered sample was gently ground using an agate mortar and pestle to ensure uniform particle size and then mounted onto a low-background sample holder. The surface was flattened to minimize preferred orientation effects prior to analysis [7]. The diffraction data were collected over a 2θ range of 10°–80° using a step size of 0.02° and a scanning speed of 2°/min under standard laboratory conditions. The operating voltage and current were maintained at 40 kV and 30 mA, respectively. Phase identification and qualitative analysis were performed using SmartLab Studio II, specifically the Search/Match (Qualitative Analysis) module, by comparing the obtained diffraction peaks with standard reference patterns from the International Centre for Diffraction Data (ICDD) database. The resulting diffractogram was used to confirm the crystalline phase of CaCO3 and to identify its polymorphic form(s) (e.g., calcite, aragonite, or vaterite). The average crystallite size was estimated using the Scherrer equation based on the most intense diffraction peaks. Fourier transform infrared (FTIR) spectroscopy analysis The FTIR analysis to detect functional groups and chemical bonding of the synthesized CaCO3NPs wereconducted using a Agilent Cary 630 FTIR Spectrometer (Manufacturer: Agilent Technologies), operated with MicroLab FTIR Software. 3 mg of the finely ground CaCO3NPs was directly placed onto the attenuated total reflectance (ATR) crystal. The sample was gently pressed to ensure good contact with the crystal surface for optimal signal acquisition. The spectra were recorded over a wavenumber range of 4000–400 cm⁻1 with a resolution of 4 cm⁻1, and 32 scans were accumulated for each measurement to improve the signal-to-noise ratio. A background spectrum was collected prior to sample analysis under identical conditions and automatically subtracted. X-ray fluorescence (XRF) analysis The elemental composition of the synthesized CaCO3 nanoparticles was determined using an energy-dispersive X-ray fluorescence spectrometer, Xenemetrix X-Calibur EDXRF Spectrometer (Manufacturer: Xenemetrix), operated with XRS-FP Analysis Software (CrossRoads Scientific). About 0.5 g of the dried sample of the CaCO3NPs was finely ground and pressed into a uniform pellet using a hydraulic press to ensure a smooth and homogeneous surface suitable for analysis. The pelletized sample was placed in the sample holder and analyzed under ambient conditions. The instrument was calibrated using appropriate standard reference materials prior to measurement. Elemental analysis was performed over a broad energy range to detect both major and trace elements present in the sample. Each measurement was conducted with an acquisition time of 120–300 s to ensure sufficient counting statistics. The obtained spectra were processed using the fundamental parameters method embedded in the analysis software to quantify the elemental composition. Scanning electron microscopy and energy dispersive X-ray (SEM–EDX) analysis The morphology and elemental composition of the synthesized CaCO3 nanoparticles were examined using a Phenom Desktop SEM equipped with an energy dispersive X-ray (EDX) detector (Phenom XL G2 SEM). About 5 mg of the dried calcium carbonate nanoparticle (CaCO3NPs) sample was evenly dispersed onto a carbon-coated aluminum stub. The sample was gently pressed to ensure proper adhesion and minimize particle agglomeration. The sample was sputter-coated with a thin layer of gold to enhance conductivity and improve image quality. The SEM analysis was conducted under high vacuum conditions at an accelerating voltage of 10–15 kV. Micrographs were obtained at different magnifications to evaluate the surface morphology, particle size, and degree of agglomeration of the nanoparticles. For elemental analysis, EDX measurements were performed at selected regions of the sample. The spectra obtained were used to identify and quantify the elemental composition of the nanoparticles. X-ray photoelectron spectroscopy (XPS) analysis The surface chemical composition and oxidation states of the synthesized CaCO3 nanoparticles were analyzed using an Kratos AXIS Ultra DLD X-ray Photoelectron Spectrometer. Approximately 103 mg of the finely powdered sample was mounted onto a conductive carbon tape attached to the sample holder. The sample surface was gently pressed to ensure uniform distribution and good electrical contact, thereby minimizing charging effects during analysis. The measurements were carried out under ultra-high vacuum conditions (~ 10⁻⁹ mbar) using a monochromatic Al Kα radiation source (hν = 1486.6 eV). Survey scans were recorded over a binding energy range of 0–1200 eV, followed by high-resolution scans for Ca 2p, C 1 s, and O 1 s, to determine their chemical states. Charge neutralization was applied during analysis to compensate for surface charging, and all spectra were calibrated with respect to the C 1 s peak at 284.8 eV. The obtained spectra were processed using appropriate background subtraction and peak fitting procedures to deconvolute overlapping peaks and assign chemical states. Thermogravimetric analysis (TGA) The thermal stability and decomposition behaviour of the synthesized CaCO3 nanoparticles were evaluated using a PerkinElmer TGA 4000 Thermogravimetric Analyzer equipped for simultaneous thermogravimetric (TGA) and differential thermal analysis (DTA). About 8.0 mg of the dried nanoparticle sample was accurately weighed and placed in a platinum crucible. The analysis was performed under a nitrogen atmosphere at a flow rate of 20 mL/min to minimize oxidative effects. The sample was programed at a constant heating rate of 10 °C/min to progressively raised the temperature from 30 °C to 900 °C. The TGA curve was used to monitor weight loss as a function of temperature, while the DTA curve provided information on the corresponding thermal events (endothermic and exothermic transitions). The prominent weight loss observed at elevated temperatures, accompanied by an endothermic peak in the DTA curve, was attributed to the thermal decomposition of CaCO3 into calcium oxide (CaO) and carbon dioxide (CO2). This thermal behaviour was used to confirm the composition and assess the thermal stability of the synthesized nanoparticles. BET surface area analysis Surface analysis of the nanoparticles for BET surface area, pore size and other properties were carried out using a Quantachrome Nova 4200e Surface Area Analyzer. The analysis was conducted using approximately 0.20–0.30 g of the dried sample. The sample was weighed into the sample tube and degassed under vacuum at 120 °C for 5 h to remove moisture and adsorbed gases. Nitrogen adsorption–desorption measurements were carried out at 77 K. The specific surface area and other properties were calculated using various adsorption isotherms such as BET and density function theory ( DFT) isotherms. Electrochemical investigations The electrochemical measurements were performed using a conventional three-electrode cell configuration connected to a computer-controlled potentiostat/galvanostat (specify model and manufacturer). The working electrode was prepared by coating a conductive substrate with a thin film of automobile welding waste deribed calcium carbonate nanoparticles (CaCO3NPs). To prepare the working electrode, a known amount of CaCO3NP powder was dispersed in ethanol containing 5 wt% polyvinylidene fluoride (PVDF) as a binder, followed by sonication for 30 min to obtain a uniform slurry. The slurry was drop-cast onto a polished glassy carbon disk electrode (diameter 3 mm) and allowed to dry under ambient conditions. The electrode surface was then gently rinsed with deionized water to remove loosely bound particles and dried before use. The geometric surface area of the coated electrode was recorded for capacitance calculations. A platinum wire served as the counter electrode, while an Ag/AgCl (3 M KCl) electrode was used as the reference electrode. All potentials were reported for this reference. The electrolyte was 0.5 M H2SO4, prepared from analytical-grade concentrated sulphuric acid diluted with deionized water. Before each measurement, the electrolyte was deaerated by purging with nitrogen gas for at least 15 min to minimize dissolved oxygen interference. Electrochemical impedance spectroscopy (EIS) was conducted over a frequency range from 105 Hz to 10⁻2 Hz with an AC perturbation amplitude of 10 mV (rms) superimposed on the open-circuit potential. The impedance spectra were recorded as Nyquist, Bode, phase angle, and imaginary impedance plots, from which relevant electrochemical parameters were extracted according to Eqs. (18)–(26). Capacitance–frequency measurements were obtained from the imaginary component of the impedance at each frequency, enabling analysis of frequency-dependent dielectric and interfacial properties. All measurements were conducted at room temperature (25 ± 2 °C). Each experiment was repeated at least three times to ensure reproducibility, and representative data are reported. Results and discussion Ultraviolet–visible spectroscopic analysis Figure 1a shows the Ultraviolet visible spectrum of the produced CaCO3NPs, while the Tauc’s plot based on the observed absorption data is provided as Fig. 1b. The observed steep rising in both the UV/Vis and Tauc’s plot, supports a well-defined indirect electronic transition, low defect and high crystallinity [36]. The shape of the graph also provide evidence of strong quantum confinement (arising from small particle sizes), concerning the deviation of the optical properties of CaCO3NPs compared to what is expected for bulk CaCO3 [17].Fig. 1a UV visible spectrum of CaCO3NPs b Tauc’s plot for indirect bandgap of CaCO3NPs a UV visible spectrum of CaCO3NPs b Tauc’s plot for indirect bandgap of CaCO3NPs The absorption spectrum shown as Fig. 1a, reveals that maximum absorption occurs at 206 nm, which indicates that the band gap calculated through the Planck equation (Eq. 2) is 6.01 eV [14].2\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${E}_{BG}= \frac{hc}{{\uplambda}_{max}}$$\end{document} Equation 1 relates the bandgap (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${E}_{BG}$$\end{document}) with the Planck constant (h), the speed of light (c) and the wavelength of maximum absorption ( \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\uplambda}_{max}).$$\end{document} In addition, the Tau’s plot was also employed to test and obtained the \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${E}_{BG}$$\end{document} of the CaCO3NPs. The Tau’s approached is based on the general equation, given as \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\left(\alpha hv\right)}^{n}=A\left(hv- {E}_{BG}\right)$$\end{document}. In this equation, α = absorption coefficient, \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\boldsymbol{h}}{\boldsymbol{v}}$$\end{document} = photon energy, A = material-dependent constant and n = exponent that depends on the type of electronic transition (Andrade et al., 2025). Consequently, possible transitions are direct allowed, direct forbidden, indirect allowed and indirect forbidden with n values equal to 2, 3/2, ½ and 1/3 respectively (corresponding to Eqs. 3–6 respectively) [6]3\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\left(\alpha hv\right)}^{2}=A\left(hv- {E}_{BG}\right)$$\end{document}4\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\left(\alpha hv\right)}^\frac{3}{4}=A\left(hv- {E}_{BG}\right)$$\end{document}5\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\left(\alpha hv\right)}^\frac{1}{2}=A\left(hv- {E}_{BG}\right)$$\end{document}6\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\left(\alpha hv\right)}^\frac{1}{3}=A\left(hv- {E}_{BG}\right)$$\end{document} The fitting of experimental data according to the above equations indicated that indirect bandgap (Fig. 1b) with a\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${E}_{BG}=5.8 eV$$\end{document}, best described the electronic transition of CaCO3NPs. This value is very close to the value (6.01 eV) obtained from Eq. 2. The slight difference between the two sets of data is because Tauc’s model is based on selectivity between direct, indirect and forbidden bandgaps, while the Planck model is based on the overall bandgap. However, both models confirm that the nanoparticles have a relatively wider bandgap, which is typical for insulators or transparent substances. Several reports have ascertained that CaCO3NPs have an indirect bandgap because their electronic transition is fulfilled by a change in momentum, when phnons iteract (a lattice vibration) to achieve the principle of conservation of momentum [8]. The present results also suggest that the transition of electrons from the valence to the conduction band can only occur through an indirect process compared to a direct transition, where some of the electrons remain unchanged during the transition [53]. Some literature values for the bandgap of CaCO3NPs are in close alignment wth our results. For example, Hossain et al. [29] stated a direct bandgap of 6.0 eV and an indirect bandgap of about 4.4 ± 0.35 eV for CaCO3, which is in strong agreement with the present results. Also, a bandgap of 5.36 eV was reported by Ghadam & Idrees [26], who synthesized CaCO3 nanoparticles using a reverse microemulsion technique. However, lower bandgap values have been reported in some studies involving different synthesis routes or material modifications. Such as 3.36 eV reported by Ramasamy et al. [60]. On the other hand, band gap as high as 7.1 eV has been reported by Janovec et al. [31], who used advanced theoretical methods to predict this value as a representatives of of an ideal crystalline calcite with minimal structural or compositional defects. Consequently, the high bandgap (~ 6.0 eV) observed in this study is consistent with theoretical and experimental reports. The minimal deviation can be attributed to the source of the raw materials, nanoparticle size, the presence of polymorph and finely oxidised carbonate phases with reduced surface contamination. The consequence is that the formed nanoparticle may favour quantum confinement effects, depending on the particle size. This could explain the observed difference between this study and others that employed bulk or doped forms of CaCO3. The results further suggest that the CaCO3NPs may not be directly useful in optical applications but can be functional as UV blockers or in UV-based optoelectronic devices, formulation of composites, in drug delivery, energy applications, as sensors and in quantum confinement turning applications. Fourier transformed infraredI guessed spectroscopy The spectrum provided in Fig. 2a represents the FTIR of CaCO3NPs, which displayed 9 peaks, whose functional information are recorded in Table 1. The FTIR analysis indicated specific vibrational modes associated with the carbonate ion (CO32⁻) and others information, which are compare with reference data (Table 1). Peaks observed at 877.79 and 862.88 cm⁻1 are a consequence of the out-of-plane bending vibrations (ν2 mode) of the CO32⁻ [48]. This peak is narrow and is within the expected range for CO32⁻ (i.e. 850–880 cm⁻1), regarding carbonate groups in the calcite form of calcium carbonate. The narrowness of the peak suggest that the vibration is well-defined CO32⁻ and signifies a pure calcite phase.Fig. 2a FTIR spectrum and b XRD pattern of the produced CaCO3NPsTable 1FTIR absorption parameters and properties assignments for the CaCO3NPsWavenumber (cm⁻1)IntensityFunctional GroupAssignmentPeak shapeReference Value (cm⁻1)Remarks862.880.65415CO32⁻ (carbonate)Out-of-plane bending (ν2 mode)Medium, narrow850–880Common for carbonate bending, calcite form877.790.63969CO32⁻ (carbonate)Out-of-plane bending (ν2 mode)Narrow850–880Typical carbonate structures (calcite)944.880.57751Ca–OStretching vibrationsWeak, medium900–950Ca–O stretching, weaker due to impurities1149.880.90260CO32⁻ (carbonate)Symmetric stretching (ν₁ mode)Strong, narrow1080–1150Strong carbonate signature1418.250.49282CO32⁻ (carbonate)Asymmetric stretching (ν3 mode)Medium1400–1470Characteristic of CO32⁻, calcite1457.390.57538CO32⁻ (carbonate)Asymmetric stretching (ν3 mode)Medium1400–1470Asymmetric stretching of CO32⁻1507.710.63749CO32⁻ (carbonate)Asymmetric stretching (ν3 mode)Medium1470–1510Aymmetric stretch3639.750.00000O–H (Hydroxyl group)Free O–H stretchingSharp, narrow3600–3650Free OH groups, a FTIR spectrum and b XRD pattern of the produced CaCO3NPs Table 1FTIR absorption parameters and properties assignments for the CaCO3NPsWavenumber (cm⁻1)IntensityFunctional GroupAssignmentPeak shapeReference Value (cm⁻1)Remarks862.880.65415CO32⁻ (carbonate)Out-of-plane bending (ν2 mode)Medium, narrow850–880Common for carbonate bending, calcite form877.790.63969CO32⁻ (carbonate)Out-of-plane bending (ν2 mode)Narrow850–880Typical carbonate structures (calcite)944.880.57751Ca–OStretching vibrationsWeak, medium900–950Ca–O stretching, weaker due to impurities1149.880.90260CO32⁻ (carbonate)Symmetric stretching (ν₁ mode)Strong, narrow1080–1150Strong carbonate signature1418.250.49282CO32⁻ (carbonate)Asymmetric stretching (ν3 mode)Medium1400–1470Characteristic of CO32⁻, calcite1457.390.57538CO32⁻ (carbonate)Asymmetric stretching (ν3 mode)Medium1400–1470Asymmetric stretching of CO32⁻1507.710.63749CO32⁻ (carbonate)Asymmetric stretching (ν3 mode)Medium1470–1510Aymmetric stretch3639.750.00000O–H (Hydroxyl group)Free O–H stretchingSharp, narrow3600–3650Free OH groups, FTIR absorption parameters and properties assignments for the CaCO3NPs A weak Ca-O vibrational peak was observed at 944.88 cm⁻1, which is within the reference range (900–950 cm⁻1) for this bond [16]. The CO32⁻ symmetric vibration (ν₁ mode) was observed at 1149.88 cm⁻1, which is also within the reference range of 1080–1150 cm⁻1 for CO32⁻ [77]. The strong signal observed at this wave number indicates the dominance of CO32⁻ content in the nanoparticles. Asymmetric stretching mode (ν3 mode) due to the presence of CO32⁻was visible between the wavenumber range 1418.25 and 1507.71 cm⁻1 and matches the expected reference range of 1400–1510 cm⁻1 [88]. These peaks, which can be defined as medium, further provide additional confirmation for the dominance of CO32⁻ groups in the calcite form of calcium carbonate nanoparticles. Although O–H stretching vibration was observed at 3639.75 cm⁻1, suggesting the presence of free O–H stretching (having an expected reference range = 3600–3650 cm⁻1), the intensity of this peak is approximately 0.00 cm−1, indicating the presence of insignificant concentration of moisture, which may be regarded as adsorbed water. XRD crystallographic study The X-ray diffraction pattern of the CaCO3NPs is shown in Fig. 2b, while quantitative parameters deduced from the plots and from the reference database are presented in Table 2.Table 2XRD diffraction and crystalline parameters for the CaCO3NPs2θ (°)HeightIntensity, I (cps)β (°)\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${d}_{cryst}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$(nm)$$\end{document}Observed d-spacing (Å)Reference d-spacing (Å)Micro strain (ε)(hkl)JCPDS Card matching CaCO318.402822120.6014.03.083.030.00258(104)47–174328.98122670.4021.64.824.840.00169(111)41–147534.384233920.7112.22.602.590.00296(202)47–174347.391441230.7512.01.921.920.00299(113)47–174351.09173970.4321.61.7861.790.00169(024)41–1475 Table 2XRD diffraction and crystalline parameters for the CaCO3NPs2θ (°)HeightIntensity, I (cps)β (°)\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${d}_{cryst}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$(nm)$$\end{document}Observed d-spacing (Å)Reference d-spacing (Å)Micro strain (ε)(hkl)JCPDS Card matching CaCO318.402822120.6014.03.083.030.00258(104)47–174328.98122670.4021.64.824.840.00169(111)41–147534.384233920.7112.22.602.590.00296(202)47–174347.391441230.7512.01.921.920.00299(113)47–174351.09173970.4321.61.7861.790.00169(024)41–1475 XRD diffraction and crystalline parameters for the CaCO3NPs The obtained X-ray diffraction (XRD) pattern of the CaCO3NPs reveals peaks at various 2θ angles, matching the corresponding and specific crystallographic planes (hkl). A peak aligning with the (104) plane of the calcite phase of CaCO3NPs was observed at 2θ = 18.40° and matches with the JCPDS card 47–1743. Also, at 2θ = 28.98°, the peak corresponding to the (111) plane with a matching JCPDS card 41–1475 JCPDS was observed, showing a height of 122 counts and an intensity of 67 cps). This peak showed the least value for the full width at half maxima (0.40°), and the least broad peak. This peak also correspond to the calcite structure of the CaCO3NPs. At a diffraction angle of 2θ = 34.38°, a peak with a height of 423 counts and an intensity of 392 cps was observed and corresponds to the (202) diffraction plane of calcite that matches JCPDS card 47-1743. However, the peak that appeared at 2θ = 47.39°, with a height of 144 counts and an intensity of 123 cps represents the (113) plane, which aligns with JCPDS card 47-1743 for calcite. Finally, at 2θ = 51.09°, the observed peak has a height of 173 counts and an intensity of 97 cps, which are associated with the (024) plane of CaCO3NPs. The matching reference card for this peak is JCPDS card 41-1475. It is also obvious that the nanoparticles also contain trace impurities such as Si, Fe, Mg and others (as shown by SEM–EDX, XRF and XPS analyses, in the upcoming sections). However, this impurities were not indicated in the XRD spectrum because of their very low concentrations, which presented them below detection limit. The presence of trace impurities (Si, Fe, Al, Mg) can influenced crystallization by altering nucleation and growth kinetics. Mg2⁺ can stabilize vaterite by inhibiting its transformation to calcite, while Fe3⁺ and Al3⁺ introduce lattice distortion and defect sites. SiO2 may act as nucleation centers, promoting rapid formation of metastable phases. These effects explain the coexistence of calcite and vaterite. The interplanar spacing between the crystal planes (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${d}_{spacing}$$\end{document}) were calculated from the diffraction angle (θ) using the Bragg equation presented as Eq. 7 below [65].7\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${d}_{spacing}= \frac{n\lambda }{2sin\theta }$$\end{document} The order of diffraction, n, was assumed to be unity, while the wavelength of the X-ray (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\lambda $$\end{document}) is 1.5406 Å for the Cu-kα ine. The \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${d}_{spacing}$$\end{document} parameters calculated for the various diffraction angles (i.e. 2 \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\theta )$$\end{document} are provided in Table 2. The results indicate that exact matching with expected references were observed at 2 \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\theta =$$\end{document} 51.09, 47.39, and 34.38° when compared to their respective JCPDS reference card number 47–1743 for calcium carbonate. These matching further confirm that the nanoparticles represent CaCO3NPs. However, at 2 \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\theta =18.40^\circ $$\end{document}, the difference between observed and reference \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${d}_{spacing}$$\end{document} was 0.049 Å, suggesting the existence of lattice strain, impurities or slight crystal distortion in the produced CaCO3NPs. But at 2 \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\theta $$\end{document} = 28.90°, there was no significant difference between the observed and the reference \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${d}_{spacing}$$\end{document}. However, the observed imaginal difference of 0.016 Å, also confirmed the existence of minimal lattice strain in the CaCO3NPs. These observations support the fact that nanoparticles tend to show slight deviation from the reference d-spacing due to their smaller sizes, but deviation upto 5% benchmark is normally accepted as a matching signal as observed in this work [17]. Values of the full width at half maxima (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\upbeta )$$\end{document} presented in Table 2, showed a range of 0.40 to 0.75°, which confirms t hat within the crystal system, there exist different degree of peak broadening at different diffraction angles. Since this broadening is a function of crystallite size (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${d}_{(Cryst)}$$\end{document}) and macrostrain (ε), we also calculated these parameters using Eqs. 8 and 9, respectively (ref).8\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${d}_{(Cryst)}= \frac{k\uplambda }{\upbeta cos\uptheta }$$\end{document}9\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\epsilon = \frac{\upbeta }{4tan\theta }$$\end{document} The calculated values of \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${d}_{cryst}$$\end{document}, which ranged from 12.0 to 21.6 (Average = 16.28 nm), provide substantial evidence to confirm that the synthesised material has a nanoscale dimension and displayed peak broadening. Micro strain is an index that indicates the degree of lattice imperfection or distortion in nanoparticles and subsequent structural strain associated with factors such as defects or dislocations in the crystal lattice structure [83, 84]. In crystals, values of micro strain less than 0.001 are termed low, while the range, 0.001 < ε < 0.005 represents moderate stress, but high strain is associated with values greater than 0.005 [33]. Calculated macrostrain for the CaCO3NPs ranged from 0.00169 to 0.00299, which indicates that the nanoparticles have moderate micro-strain, without a highly disordered lattice system. Some consequences of the reported microstrains (moderate) can include deviation of some begaviour or parameters (such as d-spacing) from the reference standard. The calculated microstrain also suggests the the nanoparticles have appreciable active adsorption sites, which may be significant in enhancing the application of the materials (CaCO3NPs) for the adsorption removal of contaminants [72]. The observed microstrain may be consequence of the incorporation of trace concetrarion of impurities such as Mg2⁺, Fe3⁺, and Al3⁺ ions, which differ in size and charge from Ca2⁺. For example, impurities such as Mg2⁺, can stabilizes metastable CaCO3 by surface adsorption. Fe and Al ions may modify surface energy and local supersaturation, further supporting mixed-phase formation.This induces lattice distortion, contributing to peak broadening and structural defects. The crystalline phase composition of the synthesised CaCO3 nanoparticles was also analysed using the Reference Intensity Ratio (RIR) method, which is a semi-quantitative X-ray diffraction (XRD) approach. Based on the results (Table 2), two distinct polymorphs of CaCO3 were identifiable through the matching of the peak positions and intensities with th standard JCPDS cards 47–1743 and 41–1475. These peaks represent calcite and vaterite and their calculated RIR values were 5.1 and 3.1, respectively. Consequently, the weight fraction of the various phases were calculated using Eq. 10 (Li & He, 2023)10\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${W}_{i}= \frac{\frac{{I}_{i}}{RI{R}_{i}}}{\sum \frac{{I}_{i}}{RI{R}_{i}}}$$\end{document}where \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${W}_{i}$$\end{document} is the weight fraction (%) of the phase, \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${I}_{i}$$\end{document} is the intensity of the strongest diffraction peak for phase i and \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$RI{R}_{i}$$\end{document} ​ is the Reference Intensity Ratio for phase i. The result obtained shows that the CaCO3NPs consist of approximately 81% calcite and 19% vaterite with calcite as the most thermodynamically stable polymorph, having the predominant phase. The presence of vaterite, which is a metastable form, suggests that the formation conditions might have favoured rapid nucleation or local supersaturation, which are typical of vaterite stabilization [9, 23]. The occurrence of both calcite and vaterite phases is due to the Ca(OH)2 dominated composition of the precursor. \Also, the impurities presence in the materials (such as Si2+, Fe3+ and Al.2+) might have also inhibited the complete transformation of vaterite to calcite through the stabilization of intermediate polymorphs and the modification of nucleation and crystal growth kinetics [5]. Regarding long-term storage, vaterite can gradually transform into calcite under humid, thermal, or solvent-mediated conditions. However, the synthesized CaCO3NPs are expected to exhibit enhanced stability due to calcination at 650 °C, which improves crystallinity and reduces structural defects that could accelerate phase transformation. Also, storage under dry conditions can minimizes moisture-driven dissolution–reprecipitation processes. Also, the preferred orientation of the CaCO3NPs was investigated through the calculated values of the Texture Coefficient (TC) based on Eq. 11 [28]11\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$TC (hkl)= \frac{I(hkl)/{I}_{0}(hkl)}{\frac{1}{N}\sum \left(I(hkl)/{I}_{0}(hkl)\right)}$$\end{document}where \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$(hkl)$$\end{document} is the measured intensity of the diffraction peak corresponding to the (hkl) plane and \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${I}_{0}(hkl)$$\end{document} is the standard intensity of the corresponding (hkl) plane obtained from the JCPDS database. The results obtained for the various crystal planes and the associated parameters, are provided in Table 3Table 3Texture coefficient (TC) calculation for CaCO3 nanoparticles synthesized from acetylene welding wasteMiller Indices (hkl)Measured Intensity I(hkl)Standard Intensity I₀(hkl)I(hkl)/I₀(hkl)TC(hkl)(104)2121002.120.953(111)67601.120.504(202)392954.131.857(113)123502.461.106(024)97751.290.580Average I/I₀––2.224– Table 3Texture coefficient (TC) calculation for CaCO3 nanoparticles synthesized from acetylene welding wasteMiller Indices (hkl)Measured Intensity I(hkl)Standard Intensity I₀(hkl)I(hkl)/I₀(hkl)TC(hkl)(104)2121002.120.953(111)67601.120.504(202)392954.131.857(113)123502.461.106(024)97751.290.580Average I/I₀––2.224– Texture coefficient (TC) calculation for CaCO3 nanoparticles synthesized from acetylene welding waste TC is a measure of the anisotropy in the crystal growth, a reflection of the relative intensity of diffraction peaks and also an index for ascertaining the preferred crystallographic orientation in the sample [86], Also, differences in orientation can also influence the material’s surface energy, reactivity, and mechanical properties [58]. The calculated TC value, indicates that the material properties of the nanoparticles (such as diffusion, reactivity, and mechanical strength) can be significantly influenced by prevailing orientation. Generally, a TC value equal to 1 indicates a randomly oriented powder, but values greater than 1 indicate preferred orientation (texture)[22]. Based on the results shown in Table 2, the (202) plane shows a strong preferred orientation (TC = 1.857), which inidicates that the preferred direction for crystallite alignment is this direction, probably due to directional growth during nanoparticle formation. However, the (104) and (113) planes show moderate texture with TCs values equal to 0.953 and 1.106, respectively, whereas the (111) and (024) planes demonstrated less preferred orientation (suppression) with r TCs lower than unity. The observed moderate TC values may be due to the presence of impurities in the nanoparticles. The listed TC values align with the findings observed in the FTIR spectrum of the nanoparticles. The spectrum (Fig. 2a) revealed three major absorption bands that represent \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${CO}_{3}^{2-}$$\end{document} at ~ 1420–1480 cm⁻1 (asymmetric stretching, ν3), ~ 875 cm⁻1 (out-of-plane bending, ν2), and ~ 710 cm⁻1 (in-plane bending, ν4). Consequently, the intense ν4 band around 710 cm⁻1 (which is more pronounced in the calcite phase than in other polymorphs) correlates with the enhanced (202) and (113) orientations. This also suggests that the crystalline planes with high TC values is structurally aligned to the internal vibrational modes of the carbonate group, particularly those related to calcite. The absence of significant band splitting or weakening in the spectrum confirms the dominance of a single phase (calcite) in the nanoparticles. Therefore, the agreement between the high TC values for certain planes and the strong and well-defined FTIR bands(representing calcite) validates the (i) structural uniformity and phase composition of the synthesized CaCO3NPs and (ii) exhibition of both molecular and crystallographic anisotropy by the CaCO3NPs. The porosity of nanoparticles can be a significant parameter in analyzing their material behaviour and consequence applications. For example, at high porosity, the surface are of the nanoparticles is expected to be high and could enhance several electrical properties such as capacitance, mass transport, and reduce diffusion. In this study, the porosity of the CaCO3 was calculated using Eq. 12 (Eddy et al., 2025)12\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$Porosity=1- \frac{{\rho}_{bulk}}{{\rho}_{true}}$$\end{document} With a measured bulk (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\rho}_{bulk})$$\end{document} and true (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\rho}_{true})$$\end{document} density of 1.45 and 2.72 g/cm3 respectively, for the synthesized CaCO3NPs, a porosity value of 53.21% was obtained. This indicates that the CaCO3NPs have void space within their lattice structure. The observed porosity is within the expected range for mesoporous when compared with the literature, such as mesoporous silica mesoporous metal organic framework (50 to 70%) and mesoporous carbon (30 to 60%) [40, 62, 79]. This high porosity can be partly linked to the existent of the preferred growth in the nanoparticles along specific crystallographic planes, based on the calculated TC value. The mesoporous and partially agglomerated structurecan restricts ion mobility to slow the conversion of vaterite-to-calcite. Such input will compel the vaterite fraction to remain kinetically stable over extended storage periods, with only slow gradual transformation. The dominant phase of the produced CaCO3NPs (calcite) have a rhombohedral calcite structure with \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\alpha =\beta =\gamma =104.5^\circ $$\end{document} and \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$a=b=c$$\end{document} [80]. Consequently, the crystalline arrangement of the produced nanoparticles can be seen in such a manner that the carbonate ions are positioned in layers, having Ca.2+ inbetween gaps in the layer [89]. The fitness of the rhombohedral structures also requires that resulting arrangement is expected to exhibit a threshold symmetry axis that forms the hallmark of the trigonal system. In view of this, the lattice parameters for theCaCO3NPs and the volume of the crystal corresponding to each plane were obtained using Eqs. 13 and 14 [46]13\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\frac{1}{{d}^{2}}= \frac{a}{\sqrt{{h}^{2}+ {k}^{2}+ {l}_{2}+hk}} . \frac{1}{1-{cos}^{2}\alpha }$$\end{document}14\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$ {\mathrm{T}}V = \frac{{4a^{3} }}{3} \times \frac{\sqrt 2 }{{sin\left( \alpha \right)}} $$\end{document} The results of the calculations showed that the lattice parameter for the reflections, (104), (111), (202), (113) and (024) are 5.002, 5.0311, 5.009, 5.001 and 4.980 Å (average = 5.004 Å) respectively while the corresponding volume were 137.016, 137.420, 137.592, 137.049 and 135.216 Å3 respectively (total volume = 686.21 Å3). These results are in good agreement whern compared to the expected reference standard values of 4.99 Å and 680.160 Å3 for lattice parameter and volume, respectively. However, the observed deviation of 0.014 Å and 6.05 Å3 may be due to some defect, such as the presence of impurities and microstrain. The coexistence of calcite and vaterite may be advantageous for electrochemical performance. While calcite provides structural and thermodynamic stability, vaterite contributes higher surface energy and enhanced interfacial reactivity. This dual-phase structure can supports interfacial polarization and electrical double-layer formation, thereby contributing to the observed dielectric and impedance characteristics of the CaCO3NPs. Trace Fe and Mn may introduce redox-active sites that enhance surface electron transfer, while SiO2 reduces conductivity but improves structural stability. These impurities therefore influence the potential electrochemical and adsorption behaviour of the nanoparticles. XRF analysis The XRF technique was employed to reveal the composition of the CaCO3NPs and the profile obtained is shown in Table 4. The results display both elemental and oxide profiles of the nanoparticles. Calcium showed a composition of 98.407%, with its oxide, CaO, having 98.589%. However, carbon content is not indicated in the results because XRF cannot measure the concentration of carbon due to its low atomic number and absence of fluorescence, matrix effect and excitation, as well as inefficient intensity regarding XRF for carbon. Therefore, the obtained results indicate that the synthesized material is a calcium-based compound and strongly consolidate the presence of CaCO3. Silicon was observed as an impurity at 0.786%, with SiO2 at 0.682%. This low concentration may be useful in improving the applications of the nanoparticles through stabilization and subsequent benefits that can enhance some applications, such as enhancement of chemical resistance by silica hardness [71]). Other elements that were found at very low concentrations were Fe at 0.198% (0.283% as Fe2O3), whose presence may enhance the catalytic, thermal and chemical behaviour of the nanoparticles [3]. Mn, Ni, Cu and their oxides had a total concentration that is < 1% while Nb and Sn contributed < 0.2%. Co, V, Ta, P, W and Ag were absent but S was found at 0.001%, with SO3 at 0.003%.Table 4XRD compositional profiling of the CaCO3NPs based on elemental and compound positionElementComposition (%)CompoundComposition (%)Si0.786SiO20.682V0.000V2O₅0.000Cr0.001Cr2O30.002Mn0.005MnO0.007Fe0.198Fe2O30.283Co0.000CoO0.000Ni0.002NiO0.020Cu0.030CuO0.038Nb0.160Nb2O30.002W0.000WO30.000P0.000P2O₅0.000S0.001SO30.003Ca98.407CaO98.589Mg0.078MgO0.029K0.000K2O0.000Ba0.000BaO0.000Al0.248Al2O30.247Ta0.000Ta2O₅0.000Ti0.000TiO20.000Zn0.004ZnO0.017Ag0.000Ag2O0.000Cl0.000Cl0.000Zr0.000ZrO20.000Sn0.030SnO20.081Na0.000Na2O0.000 Table 4XRD compositional profiling of the CaCO3NPs based on elemental and compound positionElementComposition (%)CompoundComposition (%)Si0.786SiO20.682V0.000V2O₅0.000Cr0.001Cr2O30.002Mn0.005MnO0.007Fe0.198Fe2O30.283Co0.000CoO0.000Ni0.002NiO0.020Cu0.030CuO0.038Nb0.160Nb2O30.002W0.000WO30.000P0.000P2O₅0.000S0.001SO30.003Ca98.407CaO98.589Mg0.078MgO0.029K0.000K2O0.000Ba0.000BaO0.000Al0.248Al2O30.247Ta0.000Ta2O₅0.000Ti0.000TiO20.000Zn0.004ZnO0.017Ag0.000Ag2O0.000Cl0.000Cl0.000Zr0.000ZrO20.000Sn0.030SnO20.081Na0.000Na2O0.000 XRD compositional profiling of the CaCO3NPs based on elemental and compound position SEM–EDX analysis The EDX spectrum and the data presented in Table 4 indicated that CaCO3 nanoparticles are predominantly enriched with calcium and carbon, with atomic concentrations of 64.17% and 34.85%, respectively, which is consistent with the expected stoichiometry of CaCO3 and validates the successful formation of calcium carbonate nanoparticles. The matching weight percentages (84.30% for Ca and 14.91% for C) also confirm the dominance of calcium due to its higher atomic mass, while the presence of Si (0.32 at.%), Fe (0.23 at.%), Al (0.02 at.%) and Na (0.01 at.% as trace elements indicates minor impurities, originating from the precursor (automobile welding waste). Although these impurities are present at very low concentrations (< 1%), they may influence the physicochemical properties of the nanoparticles by introducing lattice distortions or acting as nucleation modifiers, which aligns with the structural variations observed in the XRD analysis. Also, the absence or negligible detection of other elements such as Mg, K, Ti, P, S and Cl suggests a relatively high purity of the synthesized CaCO3NPs, thereby confirming that the nanomaterial is largely rich in calcium carbonate with only minimal contamination. Compared with results from the XRF (Table 4), both methods confirmed a high concentration of Ca but in the SEM–EDX, Ca has a weight concentration of 84.30%, while in XRF, calcium oxide (CaO) showed 98.589%. The difference in concentrations is due to the differences in methodologies. XRF measures oxide forms, but SEM–EDX provides elemental data. The presence of carbon is identified in the SEM–EDX results, with an atomic concentration of 34.85%, consistent with the expected composition of calcium carbonate (CaCO3). Both analyses reveal trace concentrations of Si, Mg, Al and Fe. In the XRF data. The primary difference between the two techniques lies in their sensitivity to different elements. XRF is more accurate for heavier elements (e.g., Ca) and reports concentrations as oxides, while SEM–EDX provides direct measurements of elemental composition, including light elements such carbon. Both XRF and EDX results identified calcium as the dominant element, while the differences in concentrations for other elements reflect the inherent analytical limitations and differences in how each technique reports oxides. Figure 3 shows the SEM micrographs of the CaCO3NPs at 1000 and 500 × magnifications and at three different scales with Fig. 3a, b and c representing 150, 100 and 80 µm scales, respectively.Fig. 3SEM images of CaCO3NPs at a 500 × magnification and 150 μm b 500 × magnification and 100 μm c 1000 × magnification and 80 μm SEM images of CaCO3NPs at a 500 × magnification and 150 μm b 500 × magnification and 100 μm c 1000 × magnification and 80 μm The SEM images reveal the surface morphology of CaCO3NPs at two different magnifications (100 × and 500x) and conditions. The two micrographs show a rough and irregular surface structure that is typical of nanoparticles obtained from chemical precipitation or similar methods. Evidences of agglomeration appears visibly in the micrographs, which can be regarded as consequences of the high surface energy that can initiate clustering of nanoparticles. Also, the variations in particle size are apparent in the images taken at both 500 and 1000X magnifications. Also, at a magnification of 500x, larger clusters are apparent and are indicative of regions where smaller particles have coalesced. On the other hand, at 1000 × magnification, finer particles are viewed, suggesting a relatively wide range of particle sizes that may impact some properties such as surface area and reactivity. Despite the observed agglomeration, the nanoparticles appear to maintain a consistent structure, which suggests that the production process yielded a fairly uniform product. The roughness in texture can enhance mechanical interlocking with polymer matrices or provide reactive sites for adsorption, and may support various application areas such as fillers in polymers, adsorbents in environmental remediation and drug delivery medium. XPS spectrum Figure 4 shows the XPS spectrum of the CaCO3 nanoparticles displaued over a binding wnweft range of 0–1200 eV. The spectrum shows a prominent C 1 s (~ 285 eV) and O 1 s (~ 531–533 eV) peaks that confirm the presence of carbonate (CO32⁻) groups [12, 24]. Also, the observation of Ca 2p and Ca LMM Auger peaks in the spectru, confirm the presence of calcium as Ca2⁺, which is also consistent with CaCO3 formation (Ni, M., & [55]). Also obserced in the spectrum were low-intensity peaks attributed to trace elements, namely Si, Fe, Mg, Na, Ni and Cu, which indicate the exitence of minor concentrations of surface impurities in nanoparticles. By comparison, findings from XPS analysis are in good agreement with XRF results, which showed CaO as the dominant component (~ 98.6%) with trace SiO2, Fe2O3 and other oxides. The distinct peak detected for carbon in XPS complements the finding reported for SEM–EDX, regarding the presence of f significant levels of Ca and C contents, thereby confirming the carbonate composition that XRF cannot directly resolve. These surface-sensitive XPS observations also support the XRD results which identified predominantly calcite (~ 81%) as the predominant constituents, vaterite (~ 19%) as minor constituents and the presence of Mg2⁺, Fe3⁺, Al3⁺ and SiO2 as impurities that contributed to lattice distortion, microstrain (0.00169–0.00299), and stabilization of mixed CaCO3 polymorphs observed in the diffraction analysis.Fig. 4XPS spectrum of the CaCO3 nanoparticles XPS spectrum of the CaCO3 nanoparticles TGA/DTA analysis The thermogravimetric analysis (TGA) and differential thermal gravimetric analysis (DTG) of the produced CaCO3NPs showed results provided in Fig. 5 below. The initial weight loss (~ 3%) was observed below 200 °C. This weigh loss may fue to the removal of physically adsorbed moisture or organic matter [30] These results confirm that the nanoparticles did not have significant moisture content, which also justified the appearance of zero intensity for OH group in the FTIR results (Table 2) for the nanoparticles. The DTA also expressed similar features as shown in the observed small shallow peak. Between the temperatures of 600 and 850 °C, the TGA curve shows a sharp drop in weight while the DTG curve displays a well-defined peak that demonstrates maximum decomposition rate. Both observations are consistent with theoretical expectation, sequel to Eq. 15Fig. 5TGA and DTA of the CaCO3NPs15\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\mathrm{C}\mathrm{a}\mathrm{C}\mathrm{O}}_{3}\left(s\right) \stackrel{\Delta (600-850^\circ C)}{\to } \mathrm{C}\mathrm{a}\mathrm{O}\left(s\right)+ {\mathrm{C}\mathrm{O}}_{2}(g)$$\end{document} TGA and DTA of the CaCO3NPs According to Eq. 15, the expected weight loss should be 43.99% which is in good agreement with the weight loss calculated from the TGA plot (~ 43%). This confirms that the material represents CaCO3NPs with calculated percentage purity (using Eq. 16) of 97.75%.16\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\% purity= \frac{Theoretical \, weigh \, loss}{Observed \, weight \, loss}\times \frac{100}{1}$$\end{document} The calculated purity of 97.75%, agrees with the compositional data obtained from XRD, XRF and EDX results. However, the onset temperature observed in the TGA for the decomposition of CaCO3NPs to CaONPs (~ 650 °C) is lower than the expected value (~ 750 °C) for bulk CaCO3 because the size effect, existent of microstrain and the large surface area characterizing the CaCO3NPs might have facilitated lower temperature decomposition [87]. Therefore, the selection of 650 °C for calcination is critical, as temperatures below this threshold can result in incomplete decomposition, while higher temperatures (> 650 °C) can promote excessive grain growth, particle sintering, and a reduction in surface area. Operating at 650 °C ensures controlled decomposition, yielding nanosized crystallites with high surface reactivity and moderate porosity. At temperatures higher than 900 °C, a stable TGA plateau, without a significant mass loss, was observed. The DTG curve also returns to baseline at this temperature, which also indicates that there is no further decomposition. The xingle sharp peak pattern shown by the DTG curve, suggests that the decomposition is a single-step process void of intermediate crystalline carbonates phases, while the lower decomposition temperature (compared to the expected value for the bulk CaCO3) indicates that enhanced reactivity is expected for the CaCO3NPs compared to the bulk material. Consequently, the reaction rate follows the Arrhenius-type temperature dependence, where the activation energy is lower than the expected value for the bulk materials. The kinetic approach to the investigation of the activation rate was modelled using the Kissinger equation, expressed as Eq. 17 [20]17\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$ln\left(\frac{\beta }{{T}_{p}^{2}}\right)= \frac{{E}_{p}}{R{T}_{p}}+ ln\left(\frac{AR}{{E}_{p}}\right)$$\end{document}where \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\beta $$\end{document} is the heating rate, Ep is the activation energy, Tp is the DTG peak temperature, A is t pre-exponential factor and R is the gas constant. Based on the slope of the plot of \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$ln\left(\frac{\beta }{{T}_{p}^{2}}\right)$$\end{document} versus \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\frac{1}{R{T}_{p}}$$\end{document} for various heating rates, the Ep was obtained as 178 kJ/mol, which is in agreement with the expected value of 180 kJ/mol. However, the pre-exponential factor was calculated as \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$4.1 \times {10}^{8} {min}^{-1}$$\end{document}. Also, the enthalpy was obtained by dividing the area under the DTA curve by the calibration constant. The measured area and the calibration constant were 67 112.82 and 0.387, while the enthalpy was 173.86 kJ/mol. Based on the standard enthalpy for CaCO3, we further confirmed the purity of the nanoparticles as 97.67%, which is also in good agreement with data obtained from other methods (XRF, EDX and XRD). BET analysis The nitrogen adsorption study was carried out to evaluate surface properties of the CaCO3NPs, such as pore diameter, surface area and pore volume, using multi-BET and DFT models. To obtained the surface area of the nanoparticles, the Multi-BET model (Eq. 18) was applied [13]18\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\frac{1}{W\left({P}_{0}/P\right)}=\frac{1}{{W}_{m}C}+ \frac{C-1}{{W}_{m}C}\times \frac{P}{{P}_{0}}$$\end{document} Symbols in Eq. 18 have the following defination; W = mass of the adsorbate (g), \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${W}_{m}$$\end{document} = mass of adsorbate required for monolayer coverage (g), P = equilibrium pressure of the adsorbate, P0 is the saturation pressure of the adsorbate and C = BET constant. C is related to the energy of adsorption. A plot of \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\frac{1}{W\left({P}_{0}/P\right)}$$\end{document} versus \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${P}_{0}/P$$\end{document} was linear (as shown in Fig. 6) and demonstrated a an excellent fitness (R.2 = 0.9975) with calculated slope (= \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\frac{C-1}{{W}_{m}C}$$\end{document}) and intercept (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\frac{1}{{W}_{m}C})$$\end{document} equal to 0.018 and 0.015, respectively. Consequently, the mass of adsorbate required for a monolayer adsorption was calculated as the reciprocal of the sum of the slope and intercept, using the following equation, as shown in Eq. 17. Also, the BET constant, C was calculated using Eq. 19 while the BET surface area (\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${s}_{BET}$$\end{document}) was obtained using Eqs. 21 [34]19\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${W}_{m}= \frac{1}{Slope+Intercept}= \frac{1}{\frac{C-1}{{W}_{m}C}+ \frac{1}{{W}_{m}C}}$$\end{document}20\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$C=1+\frac{slope}{Intercept}= 1+ \frac{C-1}{{W}_{m}C} \div \frac{1}{{W}_{m}C}$$\end{document}21\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${s}_{BET}= \frac{{N}_{A}{W}_{m}\sigma }{M}$$\end{document}where \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${N}_{A}$$\end{document} is Avogadro’s number \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$({6.022 \times 10}^{23} molecules/mole)$$\end{document}, \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\sigma $$\end{document} is the cross-sectional area of the nitrogen gas (0.162 nm2 = \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${1.62 \times 10}^{-19} {m}^{2})$$\end{document} and M is the molar mass of the gas \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$(M=28.02 g/mol)$$\end{document}. With the calculated values of Wm = 30.30 cm3/g and C = 2.20, the \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${s}_{BET}$$\end{document} was obtained as 132 m2/g, which is higher than some reported values such as 65 m2/m [70], and 42.88 m2/g [82], However, they are within the range reported by others such as 39 to 234 m2/g [32], 134.09 m2/g [68], 220.90 m2/g [35] and 260 m2/g [30]. Therefore, the produced nanoparticles show properties that are better than those from some existing sources and comparable to others, suggesting that they may be suitable for some applications, such as those related to adsorption.Fig. 6BET plot for the produced nanoparticles BET plot for the produced nanoparticles The density functional theory (DFT) model was also employed to calculate pore diameter, surface area, and pore volume. Four plots were developed from the DFT data, which were (i) Pore size distribution plot (i.e., differential volume versus pore diameter-Fig. 7a) (ii) Cummulative area distribution plot (i,e differential surface area versus pore diameter- Fig. 7b) (iii) cumulative pore volume versus pore diameter (Fig. 7a) and (iv) cumulative surface area versus pore diameter plot (Fig. 7b).Fig. 7DFT plots for CaCO3NPs based on a the variation of cumulative surface area/volume with pore diameter and b differential surface area/volume versus pore diameter DFT plots for CaCO3NPs based on a the variation of cumulative surface area/volume with pore diameter and b differential surface area/volume versus pore diameter Figure 7a indicates that both the cumulative surface area and volume available for adsorption increase with an increase in surface area and volume, respectively. The two plots are parallel to each other and suggest that the mechanism of adsorption is similar, irrespective of the volume or surface area. The observed trend also indicates that more volume and surface area are available for adsorption as the pore diameter increases, supporting the presence of enriched pore structure (observed in the porosity value) and large adsorption capacity (observed from mult-BET data). The plots (Fig. 7a) shows that the initial region is flat which points towards the presence of smaller or closed pores. After this region, the observed sharp rise suggests the presence of larger or open pores. The smooth increase of both curves indicates that the pores contribute significantly to the available surface area and volume of the nanoparticles. The plots of dS(d) versus pore diameter and dV(d) versus pore diameter (Fig. 7b) demonstrate supporting evidence for the presence of multiple peaks in both curves, and that the CaCO3NPs have a range of pore sizes, which can be beneficial for various applications, such as adsorption, where a diverse range of pore sizes allows for the capture of molecules of different dimensions. From the two plots, it is evident that the pore diameter is concentrated around 2.6472, 2.3129 and 2.0208 nm, indicating that the DFT pore diameter of the nanoparticles can be estimated as 2.6472 nm. The surface area of the nanoparticles and the pore volume were also obtained by integrating the area under the respective curves in Fig. 7b according to the following Eqs. 22 and 23 [56].22\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${S}_{DFT}={\int}_{{d}_{min}}^{{d}_{max}}dS(d)$$\end{document}23\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${S}_{DFt}={\int}_{{d}_{min}}^{{d}_{max}}dV(d)$$\end{document} The solution to the above equations indicated the total DFT surface area and volume of 36.60 m2/g and 0.16678 m3/g, respectively. Therefore, the calculated surface area to volume ratio is 819.0430 /m. The DFT estimated surface area is lower than the surface area obtained from the BET (Brunauer–Emmett–Teller) method because of the following reasons (i) whereas the BET methods assumes a multilayer adsorption on a flat surface, the DFT method considers single layer adsorption and how the adsorbate interact within a confind space in a specific pore geometry (ii) DFT is more sensitive to micropores whereas the BET method may overestimate the surface area of microporous materials. However, the two methods are in support of a very high surface area and near microporous nature of the synthesized CaCO3NPs. Electrochemical analysis The equivalent circuit model used to fit the electrochemical impedance spectroscopy (EIS) data is presented in Fig. 8. The model consists of two parallel resistor–constant phase element (R–CPE) units connected in series, representing the high-frequency (grain boundary/interfacial) and low-frequency (charge transfer) processes observed in the system. The equivalent circuit can be represented as: (R₁‖CPE₁) – (R2‖CPE2), where R₁ and CPE₁ correspond to the high-frequency process, while R2 and CPE2 describe the low-frequency charge transfer process.Fig. 8Equivalent circuit mode used to fit the EIS data Equivalent circuit mode used to fit the EIS data The electrochemical impedance spectroscopy (EIS) results for the calcium carbonate electrode in sulphuric acid solution are shown in Fig. 9a–d, while parameters deduced from the plots are recorded in Table 5. The Nyquist plot in Fig. 9a shows two distinct depressed semicircles, the smaller and larger semicircles representing observation in the high-frequency and low-frequency regions, respectively. This implies that the reactions between the electrolyte and CaCO3NPs electrode system is not a single electrochemical process. The high-frequency arc is connected to interfacial or grain boundary processes, while the low-frequency arc is associated charge transfer process at the electrode/electrolyte interface [4].Fig. 9Variation of a \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${Z}_{imag}$$\end{document} with \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${Z}_{real}$$\end{document}, b \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${Z}_{real}$$\end{document} with \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$log(f)$$\end{document}, c \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${-Z}_{mod}$$\end{document} with \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$log(f)$$\end{document} and \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${Z}_{real}$$\end{document} with \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$log(f)$$\end{document} for electrochemical behavior of CaCO3NPs produced from automobile welding wasteTable 5SEM–EDX results for analysis of CaCO3NPsEDX spectrumElementSymbolAtomicConcWeightConcCa64.1784.30C34.8514.91Al0..020.10Na0..010.01Si0.320.25Fe0.230.43Mg0.000.00K0.000.00Ti0.000.00P0.000.00S0.000.00Cl0.000.00 Variation of a \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${Z}_{imag}$$\end{document} with \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${Z}_{real}$$\end{document}, b \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${Z}_{real}$$\end{document} with \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$log(f)$$\end{document}, c \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${-Z}_{mod}$$\end{document} with \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$log(f)$$\end{document} and \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${Z}_{real}$$\end{document} with \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$log(f)$$\end{document} for electrochemical behavior of CaCO3NPs produced from automobile welding waste Table 5SEM–EDX results for analysis of CaCO3NPsEDX spectrumElementSymbolAtomicConcWeightConcCa64.1784.30C34.8514.91Al0..020.10Na0..010.01Si0.320.25Fe0.230.43Mg0.000.00K0.000.00Ti0.000.00P0.000.00S0.000.00Cl0.000.00 SEM–EDX results for analysis of CaCO3NPs The extracted electrochemical parameters (Table 6) are consistent with values reported for CaCO3-based and conventional dielectric materials. Charge transfer resistance values in the range of 10⁶–10⁷ Ω observed in this study are comparable to those reported for insulating carbonate systems, confirming the highly resistive and non-faradaic nature of the material.Table 6Electrochemical parameters deduced from Fig. 7ParametersEquationHigh frequency peakLow-frequency peak\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${R}_{ct}={\left|{Z}_{rea}\right|}_{low f}-{\left|{Z}_{real}\right|}_{hig f} ($$\end{document} Ω)(24)\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$4.0 \times {10}^{6}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$2.4 \times {10}^{7}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${f}_{max}$$\end{document}(Hz)(25)10.0031,623\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$C=\frac{1}{2\pi {f}_{max}R}$$\end{document}(26)\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$3.98 \times {10}^{-9}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$2.10 \times {10}^{-13}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\tau =\frac{1}{2\pi {f}_{max}}$$\end{document}(s)(27)0.0165.03 × 10−6\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\theta}_{min}$$\end{document}(°)(28)43.0073.00\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$n= \frac{{\uptheta}_{min}}{-90^\circ }$$\end{document}(29)0.380.81\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$Q=\frac{1}{2\pi {\left({f}_{max}\right)}^{n}{R}_{ct}}$$\end{document}(30)\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$1.66 {10}^{-8}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$1.36 \times {10}^{-12}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${C}_{dl}=Q\times {\left({R}_{ct}\right)}^{1-n}$$\end{document}(μF)(31)204.0034.30 Table 6Electrochemical parameters deduced from Fig. 7ParametersEquationHigh frequency peakLow-frequency peak\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${R}_{ct}={\left|{Z}_{rea}\right|}_{low f}-{\left|{Z}_{real}\right|}_{hig f} ($$\end{document} Ω)(24)\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$4.0 \times {10}^{6}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$2.4 \times {10}^{7}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${f}_{max}$$\end{document}(Hz)(25)10.0031,623\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$C=\frac{1}{2\pi {f}_{max}R}$$\end{document}(26)\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$3.98 \times {10}^{-9}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$2.10 \times {10}^{-13}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\tau =\frac{1}{2\pi {f}_{max}}$$\end{document}(s)(27)0.0165.03 × 10−6\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\theta}_{min}$$\end{document}(°)(28)43.0073.00\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$n= \frac{{\uptheta}_{min}}{-90^\circ }$$\end{document}(29)0.380.81\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$Q=\frac{1}{2\pi {\left({f}_{max}\right)}^{n}{R}_{ct}}$$\end{document}(30)\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$1.66 {10}^{-8}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$1.36 \times {10}^{-12}$$\end{document}\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${C}_{dl}=Q\times {\left({R}_{ct}\right)}^{1-n}$$\end{document}(μF)(31)204.0034.30 Electrochemical parameters deduced from Fig. 7 The fitting parameters obtained from this equivalent circuit model (Table 6) are consistent with those calculated analytically from Eqs. (24–31), confirming the validity of the model. The resistive elements correspond to charge transfer resistance (Rct), while the constant phase elements account for non-ideal capacitive behaviour arising from surface heterogeneity and distributed relaxation processes. Equations (32–38) were employed to quantitatively extract the key electrical and electrochemical parameters governing the system from the impedance spectra. Using these relationships, resistive (Rct),, capacitive (C, Cdl)), dispersive (n, Q), and kinetic (τ, fmax​) parameters were deduced from the complementary information provided by the Nyquist, Bode, phase-angle, and imaginary impedance plots. The Nyquist representation was used to determine resistance-related quantities (Rct) associated with distinct relaxation processes, while the Bode and imaginary impedance plots enabled identification of the characteristic relaxation frequencies (fmax​) and corresponding time constants (τ). Capacitance-related parameters (C, Cdl)) were subsequently derived from the combined resistance–frequency relationships, and deviations from ideal capacitive behavior were evaluated through phase-angle analysis using the constant phase element [15, 43, 59, 73, 83, 84]32\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${R}_{ct}={Z}_{Right, intercept}-{Z}_{Left, intercept}$$\end{document}33\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${f}_{max}= \frac{1}{2\pi {R}_{ct}C}$$\end{document}34\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$C= \frac{1}{2\pi {R}_{ct}{f}_{max}}$$\end{document}35\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\tau = {R}_{ct}C$$\end{document}36\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$${\theta}_{min}= -n \times 90^\circ $$\end{document}37\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$n= \frac{\left[{\theta}_{min}\right]}{90^\circ }$$\end{document}38\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$Q= \frac{1}{{\left(2\pi {f}_{max}\right)}^{n}}$$\end{document} Within these equations, resistance terms represent the opposition to charge transfer for each electrochemical process, frequency terms correspond to the characteristic relaxation behavior of the system, and capacitance-related terms describe charge storage and interfacial polarization effects. The inclusion of the constant phase element formalism accounts for non-ideal and dispersive behavior arising from surface heterogeneity, grain boundary effects, and distribution of relaxation times. Collectively, the parameters obtained using Eqs. (32)–(38) provide a coherent interpretation of the impedance response, allowing clear differentiation between grain-boundary-controlled and bulk-dominated charge transport processes and offering insight into the underlying electron transfer kinetics and dielectric properties of the material. The deviation of the arcs from perfect semicircles indicates non-ideal capacitive behaviour, which can be linked to surface heterogeneity and morphological irregularities of the calcium carbonate nanoparticles [10]. The diameter of each arc along the Z′ axis corresponds to the charge transfer resistance for that process, calculated using Eq. (32) as 4.0 × 10⁶ Ω for the high-frequency process and 2.4 × 10⁷ Ω for the low-frequency process. These values reveal that the low-frequency charge transfer step is significantly more resistive, suggesting sluggish electron transfer kinetics, whereas the high-frequency grain boundary process is relatively more conductive. The Bode plot in Fig. 8b displays two distinct peaks in the impedance modulus, corresponding to the two relaxation processes observed in the Nyquist plot. The frequencies at which these peaks occur, obtained using Eq. (33), are 10.00 Hz for the high-frequency process and 31,623 Hz for the low-frequency process. These frequencies represent the fmax for each process and are directly related to the capacitances and time constants of the system. The capacitance values, determined from Eq. (34) using the respective Rct and fmax, are 3.98 × 10⁻⁹ F for the high-frequency process and 2.10 × 10⁻13 F for the low-frequency process. The higher capacitance in the high-frequency process is consistent with significant interfacial polarization at the grain boundaries, while the much lower capacitance in the low-frequency process reflects the insulating nature of calcium carbonate in bulk charge transfer. The observed charge transfer resistance values (4.0 × 10⁶–2.4 × 10⁷ Ω) show a direct relationship with the calculated microstrain of the CaCO3NPs. Higher microstrain values correspond to increased lattice distortion and defect density, which enhance electron scattering and consequently increase Rct, particularly in the low-frequency process where charge transfer is more sluggish. The phase angle versus frequency plot in Fig. 8c provides further insight into the electrochemical behaviour of the system. Two maxima are observed, located at frequencies matching the relaxation processes in the Nyquist and Bode plots. The maximum phase angles θmin, obtained from Eq. (36), are 43° for the high-frequency process and 73° for the low-frequency process. When related to the ideal cases where phase angle is − 90° for a perfect capacitor, 0° for a pure resistor, and + 90° for an inductor, these values reveal significant deviations from ideal capacitive behaviour [38]. The exponent n, calculated from Eq. (37), is 0.38 for the high-frequency process and 0.81 for the low-frequency process. These n values indicate that the high-frequency process behaves as a strongly dispersive constant phase element with substantial heterogeneity, while the low-frequency process is closer to ideal capacitive behaviour, albeit still non-ideal [37]. The imaginary impedance versus frequency plot in Fig. 8d confirms the relaxation frequencies determined from the other plots, with clear peaks at 10.00 and 31,623 Hz, which correspond to the high- and low-frequency processes respectively. These frequencies were also used in calculating the CPE magnitude Q via Eq. (38), yielding 1.66 × 10⁻⁸ S·sⁿ for the high-frequency process and 1.36 × 10⁻12 S·sⁿ for the low-frequency process. The double-layer capacitance Cdl, determined from Eq. (31), is 204 μF for the high-frequency process and 34.3 μF for the low-frequency process. The large Cdl for the high-frequency process reflects substantial double-layer formation at the grain boundaries, while the smaller Cdl for the low-frequency process aligns with the high resistance and low bulk capacitance of calcium carbonate. The relatively high double-layer capacitance (204 μF) at the high-frequency process aligns with reported values for porous dielectric fillers and nanoparticle-based systems, where enhanced surface area and interfacial polarization contribute to increased capacitance. Conversely, the lower capacitance at the low-frequency process reflects the bulk insulating behaviour typical of CaCO3 materials. The texture coefficient values also correlate with interfacial capacitance behaviour. The (202) plane, which exhibits the highest TC (1.857), is associated with enhanced grain alignment and increased surface exposure, contributing to higher double-layer capacitance (204 μF). In contrast, planes with lower TC values correspond to reduced electroactive surface area and lower capacitance, as observed in the low-frequency process (34.3 μF). The quantitative parameters from Figs. 8a–d link closely to each other and provide a coherent picture of the electrochemical behaviour. The high-frequency process is characterised by relatively low resistance, higher capacitance, larger double-layer capacitance, and a low n value, pointing to non-ideal capacitive behaviour dominated by surface heterogeneity. In contrast, the low-frequency process exhibits much higher resistance, very low capacitance, smaller double-layer capacitance, and a higher n value closer to unity, indicating a more uniform but highly resistive charge transfer mechanism. The high Rct for the low-frequency process implies strong resistance to electrochemical corrosion in acidic medium, while the relatively high Cdl in the high-frequency process suggests potential for interfacial polarization applications. The combination of these properties confirms that calcium carbonate in this configuration behaves as a highly insulating, corrosion-resistant material with significant dielectric properties at interfaces, making it suitable as a dielectric filler, corrosion barrier, or inert electrode support in electrochemical devices. Although CaCO3 is intrinsically insulating, its electrochemical applicability extends beyond purely dielectric functions due to its significant interfacial polarization and double-layer formation. The relatively high double-layer capacitance (204 μF) observed at the grain boundary region indicates that the material can effectively support charge accumulation at the electrode/electrolyte interface, making it suitable for applications involving interfacial charge storage rather than bulk electron conduction. In such systems, CaCO3NPs function primarily as an electrochemically inactive but structurally and interfacially active material, where their high surface area, porosity, and surface heterogeneity facilitate ion adsorption, interfacial polarization, and dielectric response. These characteristics are particularly valuable in applications such as corrosion-resistant coatings, dielectric fillers, separator materials, and electrode supports. In this study, long-term cycling was not conducted, However, the high charge transfer resistance (up to 2.4 × 10⁷ Ω) and stable impedance response suggest strong resistance to electrochemical degradation and minimal faradaic activity. These characteristics indicate good inherent electrochemical stability under the tested conditions. The structural stability of the electrode is further supported by the dominance of the calcite phase, moderate microstrain, and calcination at 650 °C, which enhances crystallinity and reduces defect-driven degradation pathways. These factors collectively contribute to maintaining interfacial integrity during electrochemical measurements. Figure 10 shows the variation of capacitance with log(frequency) for the electrochemical behaviour of calcium carbonate nanoparticles in sulphuric acid solution. The plot provides complementary information to the Nyquist, Bode, phase angle, and imaginary impedance plots discussed earlier, allowing the capacitive response of the electrode to be examined directly as a function of frequency. At low frequencies, the measured capacitance is relatively high, reflecting the dominance of interfacial and double-layer charging processes where ions in the electrolyte have sufficient time to accumulate at the electrode/electrolyte interface. This behaviour is consistent with the large Cdl values previously obtained for the high-frequency process (204 μF) using Eq. (31) and reflects significant interfacial polarization at grain boundaries and surface sites of the nanoparticles. The strong frequency-dependent capacitance behaviour further supports this applicability, as the material exhibits high capacitance at low frequencies due to ion accumulation and polarization effects, despite negligible faradaic activity. This confirms that the electrochemical functionality of CaCO3NPs is dominated by interfacial and dielectric processes rather than charge transfer reactions.Fig. 10Variation of capacitance with \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$log(f)$$\end{document} for electrochemical behavior of CaCO3NPs produced from automobile welding waste Variation of capacitance with \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$log(f)$$\end{document} for electrochemical behavior of CaCO3NPs produced from automobile welding waste As the frequency increases, the capacitance decreases sharply. This is because at higher frequencies, the alternating signal changes too rapidly for complete ionic rearrangement at the interface, and the measured capacitance is increasingly determined by the dielectric properties of the electrode material itself rather than by interfacial charge storage. At very high frequencies, the capacitance approaches a constant low value, representing the intrinsic dielectric response of the calcium carbonate nanoparticles without significant contribution from faradaic or double-layer processes. This high-frequency behaviour correlates well with the extremely small capacitance values calculated for the low-frequency arc in the Nyquist plot (2.10 × 10⁻13 F from Eq. (26)), confirming that the bulk material behaves as a highly insulating dielectric at fast timescales. The combined effects of microstrain and crystallographic texture provide a structural basis for the observed impedance behaviour. Microstrain governs defect-induced resistance and charge transfer limitations, while texture coefficient controls anisotropic charge accumulation and interfacial polarization. These parameters collectively explain the dual relaxation processes observed in the impedance spectra and confirm that the electrochemical response of CaCO3NPs is intrinsically governed by their crystallographic structure. The gradual and non-ideal transition between the high- and low-capacitance regions further supports the earlier conclusion from the constant phase element exponent n (0.38 for the high-frequency process and 0.81 for the low-frequency process) that the electrode exhibits dispersive capacitive behaviour arising from surface heterogeneity and non-uniform current distribution. The reduction in capacitance with increasing frequency also aligns with the phase angle results, where the maximum values were below − 90°, indicating deviation from ideal capacitive behaviour. The observed profile in Fig. 9 therefore integrates well with the previous impedance results, confirming that the calcium carbonate nanoparticles display strong double-layer formation and polarization at low frequencies, transitioning to intrinsic dielectric behaviour at high frequencies. This frequency-dependent capacitive response highlights the suitability of CaCO3 nanoparticles for applications where high interfacial capacitance is required at slow processes, such as in protective coatings, dielectric fillers, and inert supports in electrochemical systems. Conclusion This work presents an effective synthesis of high-quality calcium carbonate nanoparticles (CaCO3NPs) from the industrial waste of oxy-acetylene gas welding in automobiles, which possess potential applications in various fields as an insulator or an interfacing material. Structural, thermal, optical, and electrochemical analyses reveal that these synthesized nanoparticles are mostly calcite and, to a smaller extent, vaterite, pure, nanometric in size, and thermally stable. Their large optical band gap and highly mesoporous nature establish the insulating properties of these particles. Electrochemical impedance spectra showed the presence of two relaxation processes associated with grain-boundary/interfacial polarization at high frequencies and bulk charge transfer processes at low frequencies. In particular, the remarkably greater charge transfer resistance for the low-frequency process (2.4 × 10⁷Ω) relative to the high-frequency process (4.0 × 10⁶ Ω) clearly reveals slow bulk electron transfer and excellent corrosion resistance in acidic solutions. In addition, high interfacial double-layer capacitance (~ 204 μF), very low bulk capacitance (≈10⁻13 F), and non-CPE behavior (n = 0.38–0.81) provide further evidence of strong dielectric and polarization contributions associated with surface inhomogeneity. The above trends of the qualitative properties and quantitative characteristics altogether make it evident that the CaCO3NPs obtained from the waste of the welding process are good insulators, corrosion resistant, and frequency-dependent with robust dielectric properties. The properties combined with its eco-friendliness make the material appropriate for use in the containing capacity of dielectric fillers, corrosion inhibitors, supporting materials for the electrode, and functional additives. The CPE exponent values (n = 0.38–0.81) are also consistent with literature reports for heterogeneous and porous dielectric systems, where deviations from ideal capacitive behaviour arise from surface roughness, grain boundary effects, and distributed relaxation times. The non-ideal capacitive behaviour described by the CPE exponent (n = 0.38–0.81) is quantitatively consistent with the measured microstrain values. Increased microstrain introduces a distribution of relaxation times due to structural disorder, which manifests as depressed semicircles in Nyquist plots and reduced phase angles, confirming dispersive charge storage behaviour. The electrochemical impedance behaviour is strongly influenced by the structural parameters obtained from XRD analysis. In particular, the moderate microstrain (0.00169–0.00299) contributes to lattice defects and surface heterogeneity, which correlate with the non-ideal capacitive response observed in EIS (n = 0.38–0.81). Similarly, variations in texture coefficient (TC) reflect anisotropic crystallographic orientation, which governs charge transport pathways and interfacial polarization behaviour. Despite the promising results, some limitations of the present study should be acknowledged. The electrochemical analysis was limited to impedance-based evaluation without long-term cycling or durability testing. In addition, detailed surface area quantification–property correlation and in-depth electrochemical performance benchmarking against standard materials were not fully explored. Future studies will focus on long-term electrochemical cycling and durability testing to further evaluate the structural and interfacial stability of the CaCO3NP-based electrodes under extended operating conditions. The need for the employment of other profiling methods such as atomic force microscopy is also proposed.