Post-explosion radiation shielding efficiency of improved reinforced concrete slabs subjected to intensive air explosions Authors: Ahmad Ramazani, Maysam Samadi, Mohammad Fayyaz, Mahdi Eshghi Published: 2026 ABSTRACT Safeguarding lives against radiations arising after an explosion near nuclear facilities has become a vital, yet underexplored concern. This requires structures with radiation shielding capabilities even after the explosion-induced damages. This paper presents the results of an experimental and analytical study on the effects of severe air explosions on concrete slabs considering two aspects of structural damage and the transmissibility of gamma and neutron particles. Initially, the ratio of neutron and gamma particles transmitted through the slab were measured. Then the slabs were subjected to air explosion, and the amount of damage was evaluated and the ratio of transmitted particles through the damaged slabs was measured. Two approaches were applied for reducing the structural damage and radiation transmissibility of these slabs, including modifying mix design with optimum combination of admixtures and an innovative core confining method. As the first approach, several combinations of minerals, fibers, heavy fine barite and B4C powder were examined to find the best mixture, in terms of compressive, tensile and flexural strengths and radiation transmissibility. As the second approach, the slab core was confined with spiral reinforcements. The results show that the modified concrete mixture could increase compressive and bending strengths up to 24% and 42% and reduce the transmission ratio of gamma and neutron about 19% and 26% in pre-blast tests, but after explosion, due to the imposed damage, its transmission ratio increased about 35%. The slab utilizing both optimal mix design and confined core showed excellent resistance against blast with negligible damage saving about 94% of its radiation-shielding efficiency after the explosion. The Tested slabs were analyzed in LS-DYNA and their response to explosion was studied. Parametric study showed the higher influence of spiral pitch rather than diameter on decreasing slab damage in terms of plastic strain. Introduction One of the most dangerous military threats is intensive explosions near reactors, nuclear facilities or even atomic airburst detonations, that imposes structural damages due to shock waves followed by radiation transmission ratio and may cause huge life losses. The dynamic forces from the blast can severely damage the structure that consequently allows ionizing radiation (gamma rays and neutrons) to pass through the structure. Consequently, designing structures with dual protective functions—structural strength and radiation shielding—is crucial for safeguarding human lives. Numerous studies have been performed to increase the radiation shielding efficacy of concrete to achieve Radiation-Shielding Concrete (RSC) that is able to attenuate both neutron and proton radiation1,2. Due to its radiation attenuation properties, RSC is widely applied in medical facilities (e.g., radiotherapy bunkers)3 and nuclear installations (reactor containment, waste storage)4 and military bunkers and command centers. Furthermore, in nuclear waste management, RSC serves as a critical containment barrier, effectively immobilizing radioactive materials and preventing environmental contamination5. The shielding effectiveness of RSC is governed by three key parameters including incident radiation intensity, material density (typically enhanced through heavyweight aggregates like barite or magnetite), and the atomic composition of constituent materials (particularly elements with high neutron absorption)6. The performance of RSC is significantly enhanced by dense natural aggregates. Some studies have used high-density aggregates such as barite (BaSO₄), colemanite (Ca₂B₆O₁₁·5 H₂O), magnetite (Fe₃O₄), and hematite (Fe₂O₃) to enhance both shielding and structural properties of concrete7,8. Barite increases concrete density to 3,500 kg/m³9 and Magnetite aggregates increase it up to 3,900 kg/m³, offering superior gamma-ray attenuation10. The highest linear attenuation coefficient (µ) has been achieved by using barite in comparison with other heavy elements such as magnetite, hematite, etc11. Some researches have tried to make ultra-high-performance concrete (UHPC) with radiation insulating qualities12,13. It usually has high compressive strength by limiting the w/c ratio to 0.2 and also employs fine particles14. Finer particles make the concrete’s internal structure more compact and lead to minimal pore percentage. Replacing the fine particles with heavyweight aggregates in the UHPC for radiation shielding, reduces the strength. The γ-ray mitigation of the high strength concrete is less than the concrete including heavyweight aggregates15. Studies of barite and magnetite substituted in RSC have reported improvements in tensile strength, compressive strength, and gamma-ray absorption16,17. It has been reported that the strength of high strength concrete is greatly influenced by the aggregate types, while changing aggregate type has minimal effect on normal concrete18.It has also been reported that steam curing, by optimizing the microstructure of barite radiation shielding concrete, significantly increases its mechanical strength and resistance to high temperatures19. Several attempts have been made by the researchers to increase the shielding capability of concrete against gamma and neutron radiation by adding various chemical materials. They have reported positive effect of lead oxide, nanopolymer particles containing PbO-H3BO3 and B4C on reducing the radiation absorption half-value layer20,21. The evaluation of the protective properties of reactor concrete against radiation has shown the positive results of using magnetite and barium in cement and aggregates in absorbing gamma and neutrons22. Concrete with up to 50% B4C per cement outperforms a mix without B4C in terms of compressive strength, and the mix with 75% B4C per cement has the maximum compressive strength. Boron carbide has been shown to be effective for neutron shielding23. Various methods have also been investigated to improve the mechanical properties of concrete. Their results show positive effect of fibers in increasing concrete ductility24,25, compressive strength (15–25% increase), tensile capacity (30–40% improvement), flexural performance, and material density (5–8% increase)26. Studies on the dynamic behavior of fiber concrete at high temperatures reported the positive effects of both steel and polypropylene fibers. Under dynamic loads applied to fiber concrete at high temperature, steel fibers prevent crushing into fragments and polypropylene fibers reduce the internal vapor pressure due to melting that protects the concrete microstructure27,28. In the investigation on physical and chemical attacks to reinforced concrete structures of nuclear power plants, the positive effects of adding microsilica, fly ash and metakaolin have been reported due to their proper filling role29. The resistance of concrete slabs against explosion or impact have been the subject of various studies. The use of polyisocyanate-oxazodone (PoZD) coating on square concrete slabs has increased the resistance of the slabs against contact explosion30. Some experimental and numerical researches have studied the performance of concrete slabs with various reinforcement ratios and have reported the positive effect of longitudinal reinforcements, slab depth, and the reinforcement strength on slab resistance against explosion31,32. Tensile and bending strength of concretes under impact loading have been investigated as a function of loading speed and strain rate. Results show that strength and maximum flexural deformation increase by increasing input energy and strain rate33,34. The abovementioned studies have assessed either the radiation shielding capability of intact concrete or mechanical strength of slabs against explosion. The main aim of this paper is to make a reinforced concrete slab with radiation shielding capability even after an intensive air explosion, which seems to be a critical yet underexplored risk. To achieve this aim, several improvements of concrete mix were combined with structural confinement of slab. Three reinforced concrete slabs were made, including the control specimen, the slab with improved concrete and the slab with innovatively confined core. Initially, the ratio of neutron and gamma particles transmitted through the slabs were measured and then the slabs were subjected to air explosion and the amount of damages were determined. Finally, the ratio of transmitted particles through the damaged slabs was measured after the explosion. The improved concrete included hybridized metal and polypropylene fibers with varying aspect ratios (L/D), fly ash, microsilica, Barite aggregates and B4C powder. Various combinations of minerals, fibers, heavy fine barite and boron carbide powder were examined to find the best mixture, in terms of compressive, tensile and flexural strengths. The confinement of slab core was provided by using spirals. The results show that just modifying the concrete mixture is not adequate to minimize the explosion induced damage and its consequent increased radiation transmissibility. On the other hand, the slab that utilized both optimal mix design and confined core showed excellent post-blast shielding efficiency against radiation. The studied slabs were also simulated, and their explosion resistances were also analyzed by finite element method. After validation of the models, a parametric study on the effect of the amount of confining reinforcement on the slab damage was evaluated. Experimental studies Explosion test Explosions represent an extreme form of dynamic loading characterized by exceptionally high strain rates. As classified in TM5-855-135, explosions are categorized based on their spatial relationship to structures to external explosions, that occur at a distance from structural elements, and internal explosions in direct contact with structural members. The pressure applied to concrete slabs by explosions, results in out of plane deformation in slabs. A fraction of the energy induced by the explosion is reflected and the other portion is absorbed in concrete and results in damage. The damage to the reinforced concrete slabs is due to compressive crushing in one face and tensile cracking in the other face, accompanied by considerable deformations. In addition to the crack and crushing, fragmenting is also observed when a slab is subjected to explosion36. Since the purpose of this research was investigating the effects of explosion shock waves, external explosions were imposed. The explosion tests were performed on three reinforced concrete slabs with dimensions of 40 × 40 × 10 cm3, with details shown in Fig. 1. All edges of the slab were simply supported. The slabs were reinforced with two layers of 8 mm diameter rebars spaced at 200 mm in both orthogonal directions. A load consisting of 120 g of C4 explosive, formed into a 50 mm-diameter spherical charge (equivalent to 150 g of TNT), was detonated at a standoff distance of 5 cm vertically above the top surface of the slab, as illustrated in Fig. 1. To evaluate the extent of damage to the concrete slabs, the radius and volume of the damage zone were measured and compared across the tested specimens37. Fig. 1(a) RC slab under the explosion test, (b) reinforcement detailing. (a) RC slab under the explosion test, (b) reinforcement detailing. Mechanical tests Static tests, including compressive, tensile and flexural tests were conducted on several concrete specimens to obtain the optimum mix design. The compressive strength test was performed according to B.S.1881.16 standard38 on 10 × 10 × 10 cm3 cubic specimens cured in standard conditions and tested at the age of 28 days as shown in Fig. 2a. The tensile strength test was performed according to ASTM C496 standard39 on cylindrical specimens with a height of 20 cm and diameter of 10 cm as depicted in Fig. 2b. Fig. 2Tests of mechanical characteristics of concrete specimens of first group, (a) compressive, (b) tensile and (c) flexural strength. Tests of mechanical characteristics of concrete specimens of first group, (a) compressive, (b) tensile and (c) flexural strength. Flexural strengths of beams made of various concrete mixtures were obtained using third-point loading in accordance with ASTM C1018 standard proposed for fiber reinforced concrete40. Specimens with dimensions of 10 × 10 × 50 cm3 as shown in Fig. 2c were subjected to concentrated loads at two points in the third points of the beam span. The loading continued until the specimen first crack, and the rupture modulus of each specimen was obtained. Tensile tests on reinforcements were also conducted that showed yield and ultimate strengths of 420 and 650 MPa, respectively. The same reinforcement was used for both longitudinal and spiral reinforcements. Measuring transmissibility of gamma and neutron particles Gamma and Neutron particles are uncharged particles that deeply penetrate into materials and react. The rate and type of reactions performed depend on the neutron energy and type of target material, and according to the type of reaction, the energy stored in the target material will also be different. To assess the passage rate of gamma rays and neutrons, the radioactive source was placed on one side of the reinforced concrete slab specimens and the number of gamma and neutron particles passed through the slab was counted by the detector on the other side of the slab. Neutron and gamma radiation transmission ratio tests were performed on reinforced concrete slab specimens in two phases: (1) pre-blast (undamaged state) and (2) post-blast (damaged state). These tests quantified the slabs’ shielding effectiveness by measuring particle attenuation through the slab thickness before and after explosive loading. The gamma-ray attenuation properties were characterized using a Geiger-Müller detector (Model Name, LND 712, operating voltage: 750 V). The system was calibrated prior to measurements using traceable gamma sources to ensure accurate count rate correspondence. Two standard gamma sources were employed: ¹³⁷Cs (137 µCi activity) and ³⁰Cs (30 µCi activity). All measurements were performed with a fixed source-to-detector distance. Samples were placed at five distinct irradiation points (A ~ E in Fig. 3). At each point, samples were irradiated for 180-second intervals. To establish baseline values and account for ambient radiation, background measurements (pre-blast) were conducted in triplicate at all points without the sample present, and the average background count was subtracted from all subsequent sample measurements. The results were averaged to ensure statistical reliability. In radiation physics, the half-value layer (HVL) represents the material thickness required to reduce gamma radiation intensity by 50%. The HVL was calculated using Eq. (1): Fig. 3Schematic of neutrons and gamma passing test and irradiation points; the radioactive source is attached to one side of slab and on the other side, the gamma or neutron counters are located directly in front of the source. 1\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:HVL=\frac{Ln2}{\mu\:}$$\end{document} Schematic of neutrons and gamma passing test and irradiation points; the radioactive source is attached to one side of slab and on the other side, the gamma or neutron counters are located directly in front of the source. where\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:\:\mu\:$$\end{document} is the linear attenuation coefficient (cm⁻¹), determined from the Beer-Lambert law in Eq. (2)11:2\documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:\mu\:=\frac{1}{d}ln\left(\frac{{T}_{0}}{T}\right)$$\end{document} Here, \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:d$$\end{document} is the specimen thickness (cm), \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:{T}_{0}$$\end{document} is the count rate without the material, and \documentclass[12pt]{minimal} \usepackage{amsmath} \usepackage{wasysym} \usepackage{amsfonts} \usepackage{amssymb} \usepackage{amsbsy} \usepackage{mathrsfs} \usepackage{upgreek} \setlength{\oddsidemargin}{-69pt} \begin{document}$$\:T$$\end{document} is the count rate with the material present. On the other hand, neutron counting was determined using a neutron dosimeter. This dosimeter is a high-sensitivity neutron rem meter (dose equivalent rate meter) developed by Berthold Technologies (formerly part of the former Berthold/Canberra product line). Figure 4 illustrates the experimental setup and specimen placement within the dosimeter’s measurement geometry. Fig. 4Neutron attenuation measurement test on concrete. Neutron attenuation measurement test on concrete. Description of the test results Three reinforced concrete slab specimens were made with dimensions of 40 × 40 × 10 cm3 reinforced with two meshes of 8 mm diameter rebars spaced 200 mm apart in both directions as shown in Fig. 1 and tested under air explosion. The first RC slab was made of normal concrete named as AN. The second slab was made using the optimum concrete mixture A2.C2.B of Table 9, named AEB. This optimum concrete mixture included additives like Microsilica, Fly ash, B4C powder, Barite aggregates, steel & PP fibers. The third specimen was similarly made of the optimum concrete mixture, but its core was also confined with spiral reinforcement named MEB. Table 1 summarizes the properties of these slab specimens. Table 1Summary of tested slabs characteristics.Slab nameConcrete mixture acc. to Table 9f’c (MPa)Longitudinal reinforcement (top&bot.)Confining reinforcementANNC34.5φ8@200NAAEBA2C2B53.2φ8@200NAMEBA2C2B53.2φ8@200φ8@80 spiral Table 1Summary of tested slabs characteristics.Slab nameConcrete mixture acc. to Table 9f’c (MPa)Longitudinal reinforcement (top&bot.)Confining reinforcementANNC34.5φ8@200NAAEBA2C2B53.2φ8@200NAMEBA2C2B53.2φ8@200φ8@80 spiral Summary of tested slabs characteristics. Control slab specimen with normal concrete (A.N) The first slab specimen was made with normal strength concrete and subjected to controlled explosion to evaluate blast-induced damage. The neutron and gamma transmission ratio of the slab was measured both before and after the blast. The compressive strength of the concrete used in this slab was 34.5 MPa as described in Fig. 5 and its mix ratios are summarized in Table 9. The damage state of this slab after the explosion test is shown in Fig. 5. This slab specimen experienced severe structural failure with complete fragmentation and removal of corners as well as spalling of a large deep part of the slab surface with about 25% of the specimen total volume as listed in Table 2. As a post-blast damage index, the volume of the removed concrete of each slab was measured and reported in Table 2, as the failure volume. These observations confirm the significant vulnerability of normal concrete mixtures to explosion-imposed impact loads and blast wave. Fig. 5Blast induced Damage and measuring pre and post-blast transmissibility of control Slab (A. N). Blast induced Damage and measuring pre and post-blast transmissibility of control Slab (A. N). Table 2Destruction results of ordinary reinforced slab (A.N).TypeDamage depth (cm)Diameter of failure (cm).Failure volume (cm3)Total volume (cm3)Reinforced normal slab (A.N)5024400016,000 Table 2Destruction results of ordinary reinforced slab (A.N).TypeDamage depth (cm)Diameter of failure (cm).Failure volume (cm3)Total volume (cm3)Reinforced normal slab (A.N)5024400016,000 Destruction results of ordinary reinforced slab (A.N). This figure also shows this specimen under transmissibility test before and after the explosion. In these tests, a total of 1400 gamma particles were emitted both before and after the explosion. Table 3 presents the results of gamma and neutron irradiation tests on this slab specimens. This Table lists the number of passed particles counted by the detector at five points on the opposite side as defined in Fig. 3. Post-explosion radiation transmission ratio measured at the most vulnerable point (point E), shows that almost all of the particles pass through the slab thickness. These results show the poor behavior of this slab with normal concrete against explosion and also radiation, especially after the explosion. Table 3Passed gamma and neutron in RC slab specimen AN, without slab, before and after explosion.Normal RC slab (A.N)Slab situationPoint APoint BPoint CPoint DPoint EGamma-rayWithout slab----1400Before explosion510512586548586After explosion----1366NeutronWithout slab----58Before explosion21---20.4 Table 3Passed gamma and neutron in RC slab specimen AN, without slab, before and after explosion.Normal RC slab (A.N)Slab situationPoint APoint BPoint CPoint DPoint EGamma-rayWithout slab----1400Before explosion510512586548586After explosion----1366NeutronWithout slab----58Before explosion21---20.4 Passed gamma and neutron in RC slab specimen AN, without slab, before and after explosion. RC slab with optimum concrete (AEB) Considering the poor behavior of the slab with normal concrete, improving the concrete mixture was considered as the first method to reduce the explosion-imposed damage and also enhance the pre and post explosion radiation shielding properties of the slabs. An experimental program was designed to achieve improved concrete mixture by performing compressive, tensile and bending tests on numerous concrete specimens. Almost all of the additives described in review part of the paper were used to achieve RSC were applied, including use of heavy weight aggregates, adding special neutron absorbing materials and steel and polypropylene fibers. The mixture with the best mechanical properties was used to make the second slab specimen named as AEB. In the following sections, the mix ratios of the improved and normal concrete are presented, accompanying with their obtained mechanical properties. Concrete ingredients Aggregates The aggregates used in this research include coarse aggregates with a maximum nominal size of 19 mm (3/4-inch sieve) and twice-washed fine aggregates with a maximum size of 4.75 mm. Instead of conventional natural sand used in normal concrete as fine aggregates, in the improved concrete, high-purity barite aggregates were also used as fine aggregates. Barite aggregates have been reported to improve mechanical properties and radiation shielding performance of high-strength concrete, in terms of attenuation coefficient (µ)11. The alternative barite fine aggregates used in improved mixes were proportioned such that the final gradation curve remains the same as that of the normal concrete. The physical properties of all aggregates are presented in Table 4, with particle size distributions shown in Fig. 6. Figure 7 shows the applied fine aggregates. Fig. 6Aggregate gradation curve. Aggregate gradation curve. Fig. 7Applied fine aggregates, (a) normal sand, (b) barite fine aggregates. Applied fine aggregates, (a) normal sand, (b) barite fine aggregates. Table 4Physical properties of aggregate.QuantityMixture groupNormalContaining bariteCoarse aggregates density (kg/m3)2429-Fine aggregates density (kg/m3)25803727Fine aggregate water absorption0.008%1%Coarse aggregate water absorption0.04%-Fineness modulus2.8%2.8%Fine aggregates SE0.80.85 Table 4Physical properties of aggregate.QuantityMixture groupNormalContaining bariteCoarse aggregates density (kg/m3)2429-Fine aggregates density (kg/m3)25803727Fine aggregate water absorption0.008%1%Coarse aggregate water absorption0.04%-Fineness modulus2.8%2.8%Fine aggregates SE0.80.85 Physical properties of aggregate. Cementitious materials The applied cement in all specimens was type 2 Portland cement and used fly ash in improved concrete specimens was class F consistent with ASTM-618-CLASS F and ASTMC494-TYPE G standards. The used microsilica complied with ASTM C1240-EN 13,263 standard. Physical properties and results of chemical analysis of the applied cementitious materials are summarized in Table 5. Table 5Physical properties and results of chemical analysis of cementitious materials.ItemSiO2Al2O3Fe2O3MgONa2OK2OCaOSO3TiO2CL.O.IDensity (Kg/m3)Specific ‌Surface (m2/Kg)Cement21.304.803.553.900.180.5162.8000003150300Fly ash88.504.201.600.180.080.511.820.020.0400160012 ~ 18Microsilica900.601.200.600.300.400.50000.801.5031015 Table 5Physical properties and results of chemical analysis of cementitious materials.ItemSiO2Al2O3Fe2O3MgONa2OK2OCaOSO3TiO2CL.O.IDensity (Kg/m3)Specific ‌Surface (m2/Kg)Cement21.304.803.553.900.180.5162.8000003150300Fly ash88.504.201.600.180.080.511.820.020.0400160012 ~ 18Microsilica900.601.200.600.300.400.50000.801.5031015 Physical properties and results of chemical analysis of cementitious materials. Two types of fibers were used in concrete mixtures including steel and polypropylene fibers. Steel fibers with hooks at both ends with three different aspect ratios were applied. To assess the effect of length and diameter, two values for length and diameter of these fibers were used in the mixtures as listed in Table 6 with the physical characteristics of four types of applied fibers. Table 6Properties of steel fibers and propylene.ItemSteel 1Steel 2Steel 3PPShapehookedhookedhookedstraightLength (mm)50353512Diameter (mm)0.80.80.40.035L/D634488342Modulus of elasticity (Gpa)2002002003.5Tensile strength (Gpa)110011001100350 Table 6Properties of steel fibers and propylene.ItemSteel 1Steel 2Steel 3PPShapehookedhookedhookedstraightLength (mm)50353512Diameter (mm)0.80.80.40.035L/D634488342Modulus of elasticity (Gpa)2002002003.5Tensile strength (Gpa)110011001100350 Properties of steel fibers and propylene. Boron carbide B₄C is a neutron-absorbing ceramic compound commonly employed in concrete radiation shielding applications41. This dark powder exhibits outstanding thermal neutron absorption capabilities due to its high ¹⁰B isotope content. The most effective neutron attenuation occurs through elastic scattering interactions with light nuclei, particularly hydrogen atoms in cement hydration products and boron atoms in the B₄C lattice. It also reduces the setting time of concrete42–45. In improved concrete mixtures, boron carbide was added with physical characteristics given in Table 7. Table 7Specifications of B4C powder used.TapeSizeSpecific mass solid g/cm32.52Purity percentage99%Size≤ 250 microns Table 7Specifications of B4C powder used.TapeSizeSpecific mass solid g/cm32.52Purity percentage99%Size≤ 250 microns Specifications of B4C powder used. Superplasticizer The polycarboxylate-based superplasticizer MEGAMIX AX 1000 was employed to achieve significant water reduction while simultaneously enhancing compressive strength and improving fresh concrete workability. This high-performance admixture conforms to ASTM C494 (Type G), EN 934-2for chemical admixtures. The specifications of applied superplasticizer’s are listed in Table 8. Table 8Specifications of used superplasticizer.ItemSizeSpecific mass kg/m31100percentage of aeration≥ 2%PH7 ± 1 Table 8Specifications of used superplasticizer.ItemSizeSpecific mass kg/m31100percentage of aeration≥ 2%PH7 ± 1 Specifications of used superplasticizer. Examined concrete mixtures Attempts to achieve improved concrete to enhance the slab performance against explosion and radiation, were conducted in two phases. The design of mix ratios of the specimens of the first phase that included various steel and polypropylene fibers was performed according to ACI 211.4R standard as presented in Table 946. After determining the optimal percentage and length to diameter ratio of fibers from the results of the first group of specimens, this optimal percentage was used in the mix design of the second group of specimens, in which fine aggregates of barite and with B4C powder were added to the mixture. To decrease the radiation transmissibility of concrete, it is preferred to use these materials in the form of fine aggregates to fill the matrix more uniformly. Therefore, heavy minerals of barite were used to replace a specific portion of fine aggregates of the optimal mixture of the first group for protection against gamma rays. To provide protection against neutron, B4C powder was also used. In concrete specimens of the first group, six mix ratios were used, including a mixture for control specimens, a mix for specimens containing mineral additives without fibers, and four mixes for specimens containing various steel and polypropylene fibers along with mineral additives. To obtain the optimal ratio of length to diameter for steel fibers, three ratios of 44, 63 and 88 were assessed in three mixes. A combination of 85% of steel fibers and 15% propylene fibers was selected based on previous studies47. The appropriate amounts of fly ash, silica, and steel fiber are 15%, 12% and 1% of the total weight of used cement, respectively48. Concrete containing mineral additives without fibers was abbreviated as FS, concrete containing mineral additives and 1% steel fibers with a dimensional ratio of 63 as AC, concrete containing mineral additives and steel fibers with a dimensional ratio of 63 and polypropylene fibers as A1C, concrete containing mineral additives and steel fibers with an aspect ratio of 44 along with polypropylene fibers A2C and concrete containing mineral additives and fibers with an aspect ratio of 88 along with polypropylene fibers A3C. The mix ratios of these concrete mixes are shown in the first group category in Table 9. Table 9Concrete mix ratios of specimens.ItemConcrete of slab ANInterim concrete mixturesConcrete of slabs AEB & MEBNCSFACA1CA2CA3CNC2Ordinary fine grainA2C2Ordinary fine grainA2C2BHeavy fine grainFirst group45Second groupCement (kg/m3)500365365365365365600438438Coarse aggregate (kg/m3)106916091069106910691069106910691069Fine aggregate (kg/m3)645645645645645645645645913Water (L/m3)175175175175175175210210210Microsilica (kg/m3)06060606060-7272Fly ash (kg/m3)07575757575-9090Steel fibers (kg/m3)005042.542.542.5-46.546.5Propylene fibers (kg/m3)0007.57.57.5-13.513.5Superplasticizer(L/m3)1.51.51.51.51.51.51.81.81.8w/c0.350.350.350.350.350.350.350.350.35L/D steel fibers0063634488-4444B4C(kg)--------0.60 Table 9Concrete mix ratios of specimens.ItemConcrete of slab ANInterim concrete mixturesConcrete of slabs AEB & MEBNCSFACA1CA2CA3CNC2Ordinary fine grainA2C2Ordinary fine grainA2C2BHeavy fine grainFirst group45Second groupCement (kg/m3)500365365365365365600438438Coarse aggregate (kg/m3)106916091069106910691069106910691069Fine aggregate (kg/m3)645645645645645645645645913Water (L/m3)175175175175175175210210210Microsilica (kg/m3)06060606060-7272Fly ash (kg/m3)07575757575-9090Steel fibers (kg/m3)005042.542.542.5-46.546.5Propylene fibers (kg/m3)0007.57.57.5-13.513.5Superplasticizer(L/m3)1.51.51.51.51.51.51.81.81.8w/c0.350.350.350.350.350.350.350.350.35L/D steel fibers0063634488-4444B4C(kg)--------0.60 Concrete mix ratios of specimens. After determining the optimal mixture among the specimens of the first group based on mechanical properties, to improve the radiation protection characteristics, in the specimens of the second group, heavy mineral materials including barite and B4C powder were used as replacement of some portion of the fine aggregate. Since the compressive strengths of the specimens of the first group were slightly lower than the conventional limit of high-strength concrete, i.e. 50 MPa49, in the second mixture more cement was used and proportionally, other proportions of the mix ratio were also modified. The mix ratios of the specimens of the second group are also listed as the second group in Table 9. Normal concrete without additives is named NC2, concrete with additives A2C2, concrete containing barite A2C2B. In order to make the mix ratios comparable, the total weight of cement, microsilica and fly ash was taken fixed in tree mixes. The difference between weight of heavy fine aggregates in comparison to that of normal ones in the mix ratios is due to their different densities considering the volume equality of fine aggregate in all mixtures. Mechanical properties of examined concrete mixtures Three static tests were conducted on concrete specimens made with various mix ratios of the first group to obtain compressive strength, tensile strength and modulus of rupture. Three specimens made using each mix ratios were subjected to the above tests at the age of 28 days. Figure 8 shows the typical failure mode of these specimens, and their average results are shown in Fig. 9. In addition, impact tests by dropping weight were also conducted on the specimens made of the first group that their details are presented by the authors elsewhere46. By comparing the results obtained from specimen made of the optimum A2C concrete mixture with those of the control concrete mixture NC., it can be observed that the compressive, bending and tensile strengths have increased by 35, 23 and 11%, respectively. The results also show that steel fibers with the lowest aspect ratio cause the greatest increase in compressive strength. It is also observed that the effectiveness of fibers in increasing the compressive strength of pozzolan inclusive specimen (SF) is approximately the same as the enhancement of the control concrete by adding only pozzolan. Mineral additives (SF) could increase the tensile strength just about 8%, but improvement obtained by concurrent use of fibers and mineral additives (A2C) was about 30%, which shows the significant effect of steel fibers on tensile strength, obtained by controlling the cracks. Fig. 8Failure modes of specimens after (a) compressive, (b) bending, (c) tensile tests. Failure modes of specimens after (a) compressive, (b) bending, (c) tensile tests. On the other hand, the bending strength of concrete specimens containing mineral additives alone (SF) is about 18% greater than that of normal concrete. Adding fibers to this mineral inclusive specimen has not resulted in considerable extra increase in bending strength. It confirms the negligible effect of fibers in comparison to mineral additives in improving the flexural strength of concrete. In addition to the bonding action of the mineral additives, due to their micrometer size, they uniformly fill very small holes in the matrix, which are the initial weak point in ordinary concrete. As a result, they cause the integration of the concrete matrix and consequently improve the bending strength. Fig. 9Diagram of mechanical characteristics of specimens of first group (in MPa). Diagram of mechanical characteristics of specimens of first group (in MPa). Based on the results of the above tests on the specimens made using the first group of mix ratios, it was concluded that the mix ratios of A2C containing steel fibers with the lowest L/D ratio is the optimal mixture. This optimal mixture was further modified in the second phase by adding B4C powder and modifying the fine aggregate to achieve enhanced radiation shielding properties. Results of mechanical tests on specimens made of various mixes are summarized in Fig. 9. It shows that by using mineral additives and fibers without heavy fine aggregates (A2C2), the compressive, bending and tensile strengths increased by 19% and 38%, and 12%, respectively, when compared to the control specimen of the second group of mixtures, NC2. It is also observed that adding B4C and barite heavy mineral aggregates leads to an increase in the compressive and bending strength by 24% and 42%. Adding barite decreased tensile strength by approximately 20%. This reduction in tensile strength is probably because of less adhesion or interlock of fine aggregates to the cement slurry. By comparing the applied barite aggregates and normal sand in Fig. 7 as well as cut sections of barite-including with normal concrete specimens in Fig. 10, it can be observed that unlike the porous microstructure of ordinary sand, that allows penetration and interlock of the cement slurry, barite fine aggregates (white small aggregates in the above specimen) are smooth and solid and consequently cannot provide adequate mechanical bond with cement paste required for tensile strength. Fig. 10Comparison of the cut section of barite-including specimen(top) with normal concrete (bot.) Comparison of the cut section of barite-including specimen(top) with normal concrete (bot.) Behavior of slab with improved concrete (AEB) under explosion and radiation Following determination of the optimal concrete mixture, the reinforced concrete slab specimen (AEB) made with this optimal concrete was subjected to blast testing and radiation transmission ratio measurements. As shown in Fig. 11, considerable surface damage with significant cracks but limited concrete material separation was observed. Cracking pattern includes radial cracks propagating from the detonation epicenter toward the slab perimeter with orthogonal cracks at the slab corners. In contrast to the control slab specimen AN, the corners of this slab have not been separated. The damage was quantified by the geometry of removed concrete from the slab surface as listed in Table 10. The measurements of the neutron and gamma transmission ratio through the slab are presented in Table 11. Fig. 11Blast induced damage and measuring pre and post-blast transmissibility of optimally reinforced concrete slab (AEB). Blast induced damage and measuring pre and post-blast transmissibility of optimally reinforced concrete slab (AEB). Table 10Destruction results of ordinary reinforced slab (AEB).Damage depth (cm)Diameter of failure (cm)Failure volume (cm3)Total volume (cm3)RC slab with improved concrete (AEB)502410016,000 Table 10Destruction results of ordinary reinforced slab (AEB).Damage depth (cm)Diameter of failure (cm)Failure volume (cm3)Total volume (cm3)RC slab with improved concrete (AEB)502410016,000 Destruction results of ordinary reinforced slab (AEB). Table 11Passed gamma and neutron in RC slab specimen AEB, without slab, before and after explosion.RC slab with improved concrete (AEB)Slab situationPoint APoint BPoint CPoint DPoint EGamma-rayWithout slab----1447Before explosion458447433510476After explosion----703NeutronWithout slab----58Before explosion19---15.1 Table 11Passed gamma and neutron in RC slab specimen AEB, without slab, before and after explosion.RC slab with improved concrete (AEB)Slab situationPoint APoint BPoint CPoint DPoint EGamma-rayWithout slab----1447Before explosion458447433510476After explosion----703NeutronWithout slab----58Before explosion19---15.1 Passed gamma and neutron in RC slab specimen AEB, without slab, before and after explosion. The results indicate a significant enhancement in blast resistance in comparison to slab AN, by decreasing the volume of spalled concrete, containment of the fragmentation and crack propagation and finally preserving structural integrity. This is mainly because of the improvements provided by the applied fibers and supplementary cementitious materials, that as described in “Mechanical properties of examined concrete mixtures”, enhanced mechanical properties of concrete mix A2C2B used in this slab (including compressive, tensile and bending strengths). It seems that the fibers have successfully decreased crack propagation, and the mineral admixtures have enhanced matrix condensation and fracture toughness. The results of pre-explosion radiation shielding tests on this slab specimen in Table 11 confirms the significant attenuation effect of barite (BaSO₄) aggregates and boron carbide (B₄C) additives on both gamma and neutron radiation, when compared with those of slab AN. Boron carbide (B₄C) and barite (BaSO₄) serve complementary but distinct roles in radiation shielding concrete for mixed gamma-neutron fields. Boron carbide primarily functions as a neutron absorber, utilizing its boron-10 isotope which has a high thermal neutron absorption cross-section (≈ 3,840 barns). It absorbs thermal neutrons through the ¹⁰B(n,α)⁷Li reaction, effectively reducing neutron flux while minimizing secondary gamma-ray production. Although it offers some gamma attenuation due to its density and composition, this remains secondary to its neutron shielding capability. The material’s chemical stability, hardness, and radiation resistance make it suitable for long-term applications in nuclear reactors and spent fuel storage. Barite, in contrast, primarily acts as a gamma-ray attenuator due to its high density (3.7 g/cm³) and the presence of high-atomic number barium (Z = 56). These properties enhance photoelectric absorption and Compton scattering of gamma photons, making barite concrete ideal for gamma shielding in medical and nuclear facilities. While providing minimal neutron shielding itself, barite doesn’t significantly interfere with neutron moderation when properly combined with hydrogenous materials and neutron absorbers. In practical applications, concretes often combine barite for gamma attenuation with boron carbide for neutron absorption, sometimes supplemented with hydrogen-rich materials like polyethylene for fast neutron moderation, creating an effective composite shield for mixed radiation environments. A comparison between the transited Gamma and neutron particles before explosion through this slab and the control slab AN, shows decreased transmission ratio of about 19% and 26%, respectively. On the other hand, after the explosion, the gamma transition through the damaged slab has decreased to about 50%. This also provides further evidence of successful performance of the slab with improved concrete against explosion. Despite the marked improvement in blast resistance and shielding over slab AN, the extensive cracking observed in slab AEB underscored the necessity for additional structural measures to preserve full integrity, leading to the design of slab MEB with spiral confinement. RC slab with optimal concrete and core confinement (MEB) Concrete confinement has been studied extensively for enhancing the seismic behavior of RC members, but its application in increasing the blast-resistance is limited to the works on external confining RC columns with CFRP or steel tubes. It was assumed that confining the core of the slabs may enhance its behavior against explosion. Therefore, to minimize the third slab specimen failure and maximize its radiation attenuation, in addition to using the improved concrete (that was used in the previous slab specimen AEB), an innovative confinement was implemented in the third slab MEB as shown in Fig. 12. In this slab specimen, the overall assembly and longitudinal reinforcement were identical to the previous two specimens, the concrete was the same as the slab AEB, but it utilized six 5 cm-diameter spiral confining reinforcement placed at the slab core. The diameter of the spiral rebars was 8 mm and their pitch was 8 cm. Concrete confinement is traditionally used to resist against lateral dilation of concrete that enhances the compressive strength, ductility, toughness, and energy absorption capacity of concrete, that all of them are also beneficial against blast loads. Fig. 12Reinforcement and confinement detailing of concrete slab specimens. Reinforcement and confinement detailing of concrete slab specimens. Figure 13 shows the post-blast condition of the slab featuring both internal confinement and the optimized concrete mix. The blast test results for the confined RC slab specimen are presented in Tables 12 and 13. It is observed that this specimen exhibited no concrete crushing or spalling, along with a significant reduction in number of cracks and their lengths and widths. Although the obtained failure volume for the specimen MEB was zero, but some cracks are still observed on its surface. Fig. 13Post-blast damage assessment of internally confined RC slab (MEB). Post-blast damage assessment of internally confined RC slab (MEB). Table 12Blast performance evaluation of RC slab specimen MEB.Damage depth (cm)Diameter of failure (cm).Failure volume (cm3)Total volume (cm3)Internally confined RC slab with improved concrete (MEB)00016,000 Table 12Blast performance evaluation of RC slab specimen MEB.Damage depth (cm)Diameter of failure (cm).Failure volume (cm3)Total volume (cm3)Internally confined RC slab with improved concrete (MEB)00016,000 Blast performance evaluation of RC slab specimen MEB. Table 13Passed gamma and neutron in RC slab specimen MEB, before and after explosion.Confined optimal reinforced concrete slab (MEB)Slab situationPoint APoint BPoint CPoint DPoint EGamma-rayWithout slab----1354Before explosion422447.3420422.6430After explosion----486NeutronWithout slab----58Before explosion19---14.7 Table 13Passed gamma and neutron in RC slab specimen MEB, before and after explosion.Confined optimal reinforced concrete slab (MEB)Slab situationPoint APoint BPoint CPoint DPoint EGamma-rayWithout slab----1354Before explosion422447.3420422.6430After explosion----486NeutronWithout slab----58Before explosion19---14.7 Passed gamma and neutron in RC slab specimen MEB, before and after explosion. Successful application of the Confinement is due to three key structural functions: (1) enhancing compressive strength, (2) improving ductility and fracture toughness, and (3) maintaining structural integrity while dissipating blast energy through controlled deformation. As observed in Table 9, comparing the absorbed gamma particles out of emitted 1400 ones after and before explosion, shows that it has successfully maintained about 94% of its pre-explosion gamma absorption capacity. Comparison of the slab specimens Numerical modeling of slabs under explosion Validation of slab with normal concrete (AN specimen) In this section, a simulation of an explosion near a concrete slab is presented using the arbitrary Lagrangian-Eulerian (ALE) formulation in LS-DYNA software. The air and explosive were modeled using the Eulerian approach, while the concrete slab and rebar were considered as Lagrangian domains. The model consisted of four distinct components: air, explosive, concrete, and rebar. A 120 g spherical C4 charge was detonated 5 cm from the concrete target. Based on the results of the von Mises stress convergence study presented in Fig. 14a, a mesh with an approximate element size of 4 mm was selected for the concrete domain. This mesh size was chosen in the region where stress variations stabilized around the 4 mm resolution. For the surrounding air domain, a coarser mesh with element sizes ranging from 5 to 8 mm was generated. The boundary conditions for the concrete specimen imposed fixed vertical displacements at prescribed nodes. To minimize spurious reflections of the pressure wave, non-reflective boundary conditions were applied to the outer extents of the air domain. The behavior of the concrete material was simulated using the Continuous Surface Cover Model (*MAT_CSCM_CONCRETE, Material Model159), an energy-based damage model known for its effectiveness in capturing post-peak softening response. The rebars were modeled using the *SECTION_BEAM keyword and the burst load was defined via *INITIAL_VOLUME_FRACTION_GEOMETRY. The interaction between the rebars and the concrete, as well as the Eulerian-Lagrangian coupling, was handled using the *CONSTRAINED_LAGRANGE_IN_SOLID command. One of the notable limitations of the concrete model adopted in this application is its tendency to underpredict the extent of spalling damage. The material parameters and model coefficients used for the concrete are listed in Table 14.Figure a shows the mesh convergence graph of Fig. 14. Figure 14b shows the 3D simulation results, while Fig. 14c shows the ALE simulation result. The analysis consistently used the kilogram-millimeter-millisecond-gigapascal(kg-mm-ms-GPa)unit¬system. Fig. 14Three-dimensional visualization of: (a) Mesh convergence diagram based on von Mises stress (b) the explosive charge and concrete specimen geometry, and (c) the ALE simulation results. Three-dimensional visualization of: (a) Mesh convergence diagram based on von Mises stress (b) the explosive charge and concrete specimen geometry, and (c) the ALE simulation results. Table 14Material model and coefficients used for concrete (NC2). Component / model partLS-DYNA model / keywordKey parametersValue / descriptionConcrete*MAT_CSCM_CONCRETE (159)Density (RO)2.4 × 10⁻⁶ kg/mm³ (2400 kg/m³)Uniaxial compressive strength (FPC)42.65 MPaMaximum aggregate size (DAGG)19.5 mmErosion criterion (plastic strain)0.30Reinforcing bar*SECTION_BEAMCross-section diameter (TS1, TS2)8.0 mmExplosive (C4)*INITIAL_VOLUME_FRACTION_GEOMETRYMass120 gCharge geometrySphereSphere radius (RADIUS)25 mmAir (medium)*EOS_LINEAR_POLYNOMIALEquation of state coefficients (C4, C5)0.4Interaction & coupling*CONSTRAINED_LAGRANGE_IN_SOLIDRebar-to-concrete coupling & Lagrangian-Eulerian interactionActive Table 14Material model and coefficients used for concrete (NC2). Component / model partLS-DYNA model / keywordKey parametersValue / descriptionConcrete*MAT_CSCM_CONCRETE (159)Density (RO)2.4 × 10⁻⁶ kg/mm³ (2400 kg/m³)Uniaxial compressive strength (FPC)42.65 MPaMaximum aggregate size (DAGG)19.5 mmErosion criterion (plastic strain)0.30Reinforcing bar*SECTION_BEAMCross-section diameter (TS1, TS2)8.0 mmExplosive (C4)*INITIAL_VOLUME_FRACTION_GEOMETRYMass120 gCharge geometrySphereSphere radius (RADIUS)25 mmAir (medium)*EOS_LINEAR_POLYNOMIALEquation of state coefficients (C4, C5)0.4Interaction & coupling*CONSTRAINED_LAGRANGE_IN_SOLIDRebar-to-concrete coupling & Lagrangian-Eulerian interactionActive Material model and coefficients used for concrete (NC2). The plastic strain contours nevertheless provide a valid representation of failure patterns. The results are shown in Fig. 15, which displays the plastic strain contour at 5 milliseconds. The figure clearly demonstrates that the corner elements are eliminated from the model based on their effective plastic strain, matching the experimental observations, in which corners have been detached. In this figure, a direct comparison between test and simulation results is provided. Therefore, it may be concluded that the model has accurately predicted the damage pattern, particularly in the corner regions. Fig. 15Experimental vs. simulated damage pattern comparison. Experimental vs. simulated damage pattern comparison. To quantify the damage extent, corner regions manually removed from analysis, and the volume of lost elements was calculated and presented in Table 15. The finite element simulation exhibits an 8% error in predicting scabbed volume compared to experimental measurements. This shows the acceptable accuracy of the material model for near-surface detonation simulations of concrete structures. Table 15Damage quantification results under blast loading.Scabbed volume error percentageScabbed volume in ANALYSES (cm3)Number of destroyed elementsScabbed volume in tests (cm3)Diameter of failure (cm).Damage depth (cm)Slab specimen8366834,9344000245AN Table 15Damage quantification results under blast loading.Scabbed volume error percentageScabbed volume in ANALYSES (cm3)Number of destroyed elementsScabbed volume in tests (cm3)Diameter of failure (cm).Damage depth (cm)Slab specimen8366834,9344000245AN Damage quantification results under blast loading. Validation of slab with combination of confinement and optimized concrete (MEB specimen) Since this specimen used reinforcing fibers, the previous material model could not predict the behavior observed in the test. Therefore, material model 72 (*MAT_CONCRETE_ DAMAGE_ REL3) was used to simulate this slab. The concrete equation of state used in this simulation is given in Table 16and the concrete material model parameters are given in Table 17. In this simulation, the explosion was defined the same as the previous model, and the same settings were applied. The reinforcing bars were modeled using beam elements with 5 mm diameter circular section. For the material model, the dynamic increase factor (DIF) is incorporated as a function of strain rate. The input parameters for the material model are derived from the dynamic increase factor. This factor was defined according to the diagram of Fig. 16, that has been obtained based on the calibration with experimental test data50. Table 16Concrete equation of state in numerical model of improved concrete.EOS_Tabulated_CompactionEOS IDEOSIDb-Volumetric Strain 1EV10.0-Pressure 1C10.0GPaVolumetric Strain 2EV2-0.0001-Pressure 2C20.00145GPaVolumetric Strain 3EV3-0.0002-Pressure 3C30.00379GPaVolumetric Strain 4EV4-0.0005-Pressure 4C40.00907GPaVolumetric Strain 5EV5-0.0010-Pressure 5C50.01959GPa Table 16Concrete equation of state in numerical model of improved concrete.EOS_Tabulated_CompactionEOS IDEOSIDb-Volumetric Strain 1EV10.0-Pressure 1C10.0GPaVolumetric Strain 2EV2-0.0001-Pressure 2C20.00145GPaVolumetric Strain 3EV3-0.0002-Pressure 3C30.00379GPaVolumetric Strain 4EV4-0.0005-Pressure 4C40.00907GPaVolumetric Strain 5EV5-0.0010-Pressure 5C50.01959GPa Concrete equation of state in numerical model of improved concrete. Table 17Material model number 72.GroupLS-DYNA parameterDescriptionValueBasic identificationMIDMaterial identification7RODensity2.40 × 10⁻³PRPoisson’s ratio0.19StrengthFTUniaxial tensile strength0.0034Damage surface parametersA0Damage surface parameter a₀0.01032A1Damage surface parameter a₁0.40181A2Damage surface parameter a₂8.50 × 10⁻⁴A0YTensile damage parameter0.00846A2YTensile damage parameter0.00281A1FDamage surface parameter0.38268A1YDamage surface parameter0.47128B1Damage surface parameter b₁0.0OMEGADamage coupling parameter, ω0.0Strain rate enhancementLCRATENumber of strain rate points in the lookup table24LOCWIDTHReference length for rate effects58.50NFTSDynamic increase factor (DIF) for tensile strength at fracture13.00SlambdaScale factor for strain rate0.0lambda1 - lambda13Strain rate values (s⁻¹) for the lookup table0.0 to 1.00 × 10¹⁰eta1 - eta13Dynamic increase factors (DIF) corresponding to λ1-λ130.0 to 1.0OtherNOUTOutput option flag2.0EDROPEnergy drop (failure)0.0RSIZECharacteristic element size for scaling0.03937UCFUnit conversion factor (for RSIZE)1.45 × 10⁵ Table 17Material model number 72.GroupLS-DYNA parameterDescriptionValueBasic identificationMIDMaterial identification7RODensity2.40 × 10⁻³PRPoisson’s ratio0.19StrengthFTUniaxial tensile strength0.0034Damage surface parametersA0Damage surface parameter a₀0.01032A1Damage surface parameter a₁0.40181A2Damage surface parameter a₂8.50 × 10⁻⁴A0YTensile damage parameter0.00846A2YTensile damage parameter0.00281A1FDamage surface parameter0.38268A1YDamage surface parameter0.47128B1Damage surface parameter b₁0.0OMEGADamage coupling parameter, ω0.0Strain rate enhancementLCRATENumber of strain rate points in the lookup table24LOCWIDTHReference length for rate effects58.50NFTSDynamic increase factor (DIF) for tensile strength at fracture13.00SlambdaScale factor for strain rate0.0lambda1 - lambda13Strain rate values (s⁻¹) for the lookup table0.0 to 1.00 × 10¹⁰eta1 - eta13Dynamic increase factors (DIF) corresponding to λ1-λ130.0 to 1.0OtherNOUTOutput option flag2.0EDROPEnergy drop (failure)0.0RSIZECharacteristic element size for scaling0.03937UCFUnit conversion factor (for RSIZE)1.45 × 10⁵ Material model number 72. Fig. 16Dynamic increase factor (DIF) as a function of strain rate50. Dynamic increase factor (DIF) as a function of strain rate50. Based on the contour of plastic strain of this model, shown in Fig. 17, it is observed that no element elimination is occurred in this model, that verifies the experimentally observations for this specimen. Fig. 17Effective plastic strain and stress distribution at t = 14 ms. Effective plastic strain and stress distribution at t = 14 ms. The charts of maximum von Misses stress and the concrete plastic pressure against the time obtained for this slab model are presented in Figs. 18 and 19, respectively, respectively. It is observed that the plastic strain constantly increases after yielding, but the maximum von misses stress experiences a localized peak at about 1.5 ms and then returns to its global trend. This may be because of the following. Fig. 18Evolution of max von Mises stress with time. Evolution of max von Mises stress with time. Fig. 19Time-history of maximum plastic strain. Time-history of maximum plastic strain. validation and modeling of this slab configuration, the effects of confinement amount on the stress and plastic strain were investigated. A comparative analysis of the resulting diagrams reveals the effects of varying these parameters. The quantitative results of these modifications in spiral pitch and diameter are summarized in Table 18. Table 18Maximum plastic strain and von mises stress results for various confinement ratios.Plastic strainVon Mises stressModel nameParameter1.560.0298MEB.50 mmSpiral pitch1.660.0306MEB.80 mm1.780.0316MEB.110 mm1.640.0306MEB.6 mmSpiral diameter1.670.0306MEB.8 mm1.680.0307MEB.12 mm Table 18Maximum plastic strain and von mises stress results for various confinement ratios.Plastic strainVon Mises stressModel nameParameter1.560.0298MEB.50 mmSpiral pitch1.660.0306MEB.80 mm1.780.0316MEB.110 mm1.640.0306MEB.6 mmSpiral diameter1.670.0306MEB.8 mm1.680.0307MEB.12 mm Maximum plastic strain and von mises stress results for various confinement ratios. The parametric study revealed that spiral pitch had significantly higher influence on structural performance against explosion than spiral diameter. A 3 cm change in spiral pitch (either reduction or increase) resulted in approximately 6% change in plastic strain. In contrast, varying the spiral diameter from 6 mm to 12 mm demonstrated negligible impact on strain. These findings indicate that the spatial arrangement of confining element (pitch) is considerably more effective than its diameter for reducing the explosion-induced actions in RC slab models. Conclusions The resistance of RC slabs against air explosion and their pre and post- explosion shielding capability against neutron and gamma were experimentally studied. The RC slab with normal concrete experienced extensive damages resulting in high transmission ratio after the blast. Two other specimens were made with improved concrete components, one with traditional reinforcement and the other with additional internal confining spirals. The improved concrete mix ratio was obtained based on the results of compressive, tensile, bending and impact tests on several specimens made with various combinations of admixtures, including microsilica, fly ash, steel and polypropylene fibers, barite and B4C powder. Simulation of the studied slabs were conducted in LS-DYNA. The following conclusions may be made. Improving the slab concrete by optimal combination of used additives could significantly reduce crushing and separation of its surface, under explosion test, but still several cracks were observed. Confining the core of the slab with improved concrete could prevent surface crushing.The results of the gamma and neutron radiation tests on the slabs before the explosion indicated that the Barite and B4C powder could successfully reduce the transmission ratio of gamma and neutron about 19% and 26%, in comparison to the slab with normal concrete.After the explosion, due to the damage imposed on the slab with normal concrete, about 98% of the emitted rays passed. The slab with improved concrete containing heavy minerals passed about 50% of gamma ray. But the slab with confined core made of optimal concrete could successfully absorb about 65% of the emitted gamma ray that means it has maintained up to 94% of its pre-explosion absorption capacity.The parametric analytical study revealed that spiral pitch has significantly greater influence on structural performance than spiral diameter. Improving the slab concrete by optimal combination of used additives could significantly reduce crushing and separation of its surface, under explosion test, but still several cracks were observed. Confining the core of the slab with improved concrete could prevent surface crushing. Improving the slab concrete by optimal combination of used additives could significantly reduce crushing and separation of its surface, under explosion test, but still several cracks were observed. Confining the core of the slab with improved concrete could prevent surface crushing. The results of the gamma and neutron radiation tests on the slabs before the explosion indicated that the Barite and B4C powder could successfully reduce the transmission ratio of gamma and neutron about 19% and 26%, in comparison to the slab with normal concrete. The results of the gamma and neutron radiation tests on the slabs before the explosion indicated that the Barite and B4C powder could successfully reduce the transmission ratio of gamma and neutron about 19% and 26%, in comparison to the slab with normal concrete. After the explosion, due to the damage imposed on the slab with normal concrete, about 98% of the emitted rays passed. The slab with improved concrete containing heavy minerals passed about 50% of gamma ray. But the slab with confined core made of optimal concrete could successfully absorb about 65% of the emitted gamma ray that means it has maintained up to 94% of its pre-explosion absorption capacity. After the explosion, due to the damage imposed on the slab with normal concrete, about 98% of the emitted rays passed. The slab with improved concrete containing heavy minerals passed about 50% of gamma ray. But the slab with confined core made of optimal concrete could successfully absorb about 65% of the emitted gamma ray that means it has maintained up to 94% of its pre-explosion absorption capacity. The parametric analytical study revealed that spiral pitch has significantly greater influence on structural performance than spiral diameter. The parametric analytical study revealed that spiral pitch has significantly greater influence on structural performance than spiral diameter. On the other hand, the mechanical tests conducted to find the best mixture show that: Both steel and pp fibers and mineral additives, including microsilica and fly ash, increased compressive and tensile strengths of concrete, but mineral additives were more effective in increasing flexural strength than fibers. The steel fibers with the lowest aspect ratio result in the greatest increase of the compressive, tensile, and bending strengths. B4C and barite heavy fine aggregates increased the compressive and bending strengths. The tensile strength of the specimen containing barite slightly decreased in comparison with the control specimen, primarily due to weaker interfacial bonding between the smooth barite particles and cement paste, which reduced stress transfer efficiency under tensile loading. This study is an initial step in application of spiral confinement for enhancing blast resistance and post-blast radiation-shielding of slabs and therefore its results are limited to the specimens studied. Several parameters can be studied in more details for further development of these structures to save human lives, including mechanical properties, dimensional ratios, volumetric ratio, arrangement and direction of confining spirals.