Magnetic-Field-Enhanced Microwave Absorption of Superparamagnetic Fe3O4/RGO Composites Authors: Guijiang Liu, Xingbao Lyu, Yiqun Ma, Chengxun Yuan, Zhongxiang Zhou Published: 2026 ABSTRACT Superparamagnetic materials have attracted increasing attention for high-frequency microwave absorption because superparamagnetic relaxation can partially overcome the high-frequency limitations of conventional magnetic absorbers. Herein, Fe3O4/rGO composite powders were prepared by electrostatic self-assembly and subsequently incorporated into an epoxy matrix, and magnetic-field-induced alignment was introduced during curing. Owing to the synergistic effects of interfacial polarization, magnetic dissipation, and improved impedance matching, the optimized composites exhibited markedly enhanced microwave absorption performance. In particular, when the rGO content was 10 wt% and an external magnetic field was applied, the composite achieved effective absorption across the entire X-band (8–12 GHz) within a thickness range of 1–3 mm, together with a minimum reflection loss of −40.3 dB. The enhanced performance is attributed to the combined contributions of abundant heterogeneous interfaces, superparamagnetic relaxation, and field-induced orientation of Fe3O4-decorated rGO sheets. This work provides a simple physical strategy for the microstructural regulation of magnetic–dielectric composites toward high-performance microwave absorption. 1. Introduction The rapid advancement of electronic communication technology, while fostering significant innovation and convenience, has inevitably led to severe electromagnetic (EM) radiation pollution [1,2,3,4,5]. This issue poses serious risks to the stable operation of precision equipment and human health. Microwave absorption materials (MAMs), which integrate superior impedance matching with robust attenuation capabilities, have emerged as an effective solution to mitigate EM pollution [6,7,8]. However, most single-phase materials struggle to simultaneously achieve optimal impedance matching and high attenuation due to their intrinsic limitations. On one hand, single-component carbon materials—ranging from 0D carbon quantum dots and 1D carbon nanotubes to 2D graphene and 3D carbon foams—are often restricted by poor impedance matching and limited EM wave attenuation pathways [9,10,11,12,13]. On the other hand, magnetic materials are constrained by high density and the Snoek’s limit at high frequencies [14,15]. Consequently, there is an urgent need to explore strategies that effectively synergize the advantages of both components to develop low-density, high-efficiency MAMs. To introduce additional attenuation mechanisms and optimize impedance matching, various strategies have been proposed, among which the utilization of interfaces to enhance interfacial polarization is considered a highly attractive approach [16,17]. By incorporating magnetic phases such as Co, Ni, or Fe3O4 into carbon-based substrates (e.g., graphene, porous carbon, or carbon fibers), researchers have constructed heterogeneous magnetic-carbon interfaces [17,18,19,20]. These interfaces promote space charge accumulation and interfacial polarization loss, which, in synergy with magnetic loss, significantly improve both impedance matching and EM attenuation capacity [21]. For example, Co nanoparticle-decorated carbon nanofibers with abundant structural defects, hierarchical Co2P/CoS2@C@MoS2 composites with multiple heterointerfaces, and ion-doped hollow spinel absorbers have exhibited excellent microwave absorption performance through the synergistic regulation of conductive loss, interfacial polarization, magnetic loss, and impedance matching [22,23,24]. In recent years, superparamagnetic nanomaterials have garnered widespread attention due to their efficient microwave absorption at high frequencies. Superparamagnetic relaxation effectively overcomes Snoek’s limit, demonstrating impressive absorption performance at high microwave frequencies. For instance, Song and Zhang et al. synthesized SiO2-coated superparamagnetic Fe3O4 nanoparticles, achieving relaxation frequencies of 6.9 GHz and 9.3 GHz, respectively, through superparamagnetic coupling [14,15]. Yuan et al. anchored superparamagnetic Fe3O4 nanoparticles onto carbon nanotubes using a co-precipitation method, reaching a resonance frequency of 9.1 GHz [25]. Similarly, Anh et al. fabricated superparamagnetic Zn0.8Ni0.2Fe2O4 alloys that exhibited an absorption attenuation exceeding 20 dB at 10 GHz [26]. Under an external magnetic field, superparamagnetic nanoparticles align into chain-like structures along the field direction through magnetic dipole interactions [27]. This magnetically aligned chain-like structure provides a more efficient pathway for microwave propagation and dissipation within the absorber and is considered a reliable strategy for regulating the microwave response of magnetic fluids [28,29]. Polymer-based electromagnetic functional materials have attracted considerable attention in electromagnetic interference shielding, microwave absorption, and multifunctional electromagnetic devices owing to their low density, processability, and structural designability [30]. If a magnetic field is applied during the polymerization process, the alignment remains embedded within the composite matrix once the solvent solidifies and the field is removed. This processing technique has already been applied to enhance mechanical properties and achieve flexible robotic manipulation [31,32,33]. Meanwhile, electrostatic self-assembly is regarded as an effective strategy for inducing microstructural organization during polymer processing [34]. In this study, a facile, low-cost, and environmentally friendly method was developed to fabricate superparamagnetic Fe3O4/rGO composites. The self-assembly of superparamagnetic Fe3O4 and reduced graphene oxide (rGO) was achieved via electrostatic adsorption, leveraging the potential difference between the materials. When incorporated into an epoxy resin matrix under an external magnetic field, the rGO sheets decorated with superparamagnetic iron oxide nanoparticles (SPIONs) aligned along the field lines. By combining electrostatic assembly with magnetic-field-induced structural control, the Fe3O4/rGO composites achieved an effective absorption bandwidth (EAB) covering the entire X-band (8–12 GHz) within a thickness range of 1–3 mm, with a minimum reflection loss (RLmin) of −40.3 dB. This work demonstrates a physical approach for microstructural reassembly of nanoscale composites via electrostatic adsorption and magnetic-field induction, providing novel insights for the development of EM shielding, microwave absorption materials, and broader composite engineering. 2. Materials and Methods 2.1. Materials The Fe3O4 nanoparticles (spherical morphology, 10–20 nm in diameter) were purchased from Qinghe Xingye Metal Materials Co., Ltd. (Jinan, China). Monolayer rGO was obtained from Shenzhen Suiheng Technology Co., Ltd. (Shenzhen, China). E51 epoxy resin was supplied by Kunshan Jiulimei Electronic Materials Co., Ltd. (Kunshan, China). Standard hydrochloric acid (HCl) solution and curing agents, including diethylenetriamine (DETA) and dibutyl phthalate (DBP), were provided by Sinopharm Chemical Reagent Co., Ltd. (Shanghai, China). All reagents were used as received without further purification. 2.2. Preparation of Composite Materials The Fe3O4/rGO composite powders were synthesized via an electrostatic adsorption method. Typically, specified amounts of Fe3O4 and rGO powders were dispersed separately in deionized (DI) water. After stirring for 5 min, the mixtures were subjected to pulsed ultrasonication for 30 min to obtain 0.1 g/L dispersions of Fe3O4 and rGO, respectively. Subsequently, the pH values of the two dispersions were adjusted to 5.5–6.0 by adding a standard hydrochloric acid solution. As shown in Figure S1, at this pH, the zeta potential of the Fe3O4 nanoparticles was approximately +10 mV, whereas that of rGO was approximately −8 mV. The opposite signs of their surface charges enabled electrostatic-attraction-driven self-assembly between the Fe3O4 nanoparticles and the rGO sheets, resulting in the immobilization of Fe3O4 nanoparticles on the rGO surface. The two dispersions were then subjected to an additional 2 min of ultrasonication. Under constant magnetic stirring at 500 rpm, the rGO dispersion was added dropwise into the Fe3O4 dispersion, with the volume of the rGO dispersion controlled according to the mass ratios listed in Table 1. The resulting mixture was briefly ultrasonicated for 2 min and then stirred continuously at room temperature for 2 h to promote self-assembly. The Fe3O4/rGO composite precipitate was collected through magnetic separation, and the supernatant was discarded. The obtained precipitate was washed twice with DI water, involving 1 min of ultrasonication followed by magnetic separation for each cycle. Finally, the composites were dried in a drying oven at 50 °C for 12 h to obtain Fe3O4/rGO composite powders. The fabrication process of the Fe3O4/rGO/epoxy composites is described as follows: (1) Premixing: The as-prepared Fe3O4/rGO composite powders were mixed with epoxy resin according to the weight ratios specified in Table 1. The mixture was subjected to mechanical stirring at 500 rpm for 30 min at room temperature to ensure uniform dispersion. (2) Curing-agent Addition and Degassing: Subsequently, the curing-agent was added to the mixture at a resin-to-curing agent weight ratio of 5:1 and stirred for an additional 15 min. The resulting mixture was then allowed to stand for 10 min to remove entrapped air bubbles. (3) Casting and Magnetic Alignment: The mixture was quickly cast into customized silicone waveguide molds (fabricated via 3D printing/additive manufacturing). The internal dimensions of the molds were 22.86 × 10.16 × 2 mm (as shown in Figure S2a), corresponding to standard waveguide requirements. To induce directional alignment, the molds were placed between two square permanent magnets (50 × 50 × 20 mm). The magnetic field intensity at the sample center was measured to be 80 mT using a Gauss meter (DLX-STW1044), as illustrated in Figure S2b. (4) Curing: The samples were cured at room temperature for 6 h under the applied magnetic field. For comparison, a control group was prepared under identical conditions but without the external magnetic field. Three types of Fe3O4/rGO composites with different mass fractions were fabricated (see Table 1). The overall preparation workflow is schematically illustrated in Figure 1. 2.3. Characterization The phase compositions of the Fe3O4 nanoparticles and Fe3O4/rGO composites were analyzed by X-ray diffraction (XRD, PANalytical X’Pert PRO). The zeta potentials of the Fe3O4 and rGO powders were measured using a Zeta potential analyzer (Zeta potential, Malvern Zetasizer Nano ZSP) to determine their surface charge states. The microstructure and surface morphology of the Fe3O4 nanoparticles and the composites were characterized via scanning electron microscopy (SEM, Zeiss Gemini 560). Magnetic properties, including hysteresis loops, were investigated using a vibrating sample magnetometer (VSM, Lake Shore 7404). The electromagnetic (EM) parameters of the samples were measured in the X-band (8–12 GHz) using a vector network analyzer (VNA, Keysight PNA-L) via the waveguide method. Before testing, the VNA was calibrated using a 32118 waveguide calibration kit. 3. Results and Discussion 3.1. Composition and Structure of Composite Materials Figure 2 shows the XRD patterns of the Fe3O4 nanoparticles and Fe3O4/rGO composites. The diffraction peaks of Fe3O4 are indexed to the (111), (311), (222), (400), (422), (511), and (440) planes, which are in good agreement with the standard cubic spinel phase (JCPDS No. 19-0629). The sharp and intense peaks indicate a high degree of crystallinity in the Fe3O4 NPs. No characteristic peaks of impurities or intermediate phases were detected, confirming the high chemical and phase purity of the nanoparticles [35]. For the Fe3O4/rGO composites, the characteristic peaks of Fe3O4 remain prominent, while the appearance of the (002) plane confirms the successful incorporation of rGO [36]. As illustrated in Figure 3a, the particle size of the Fe3O4 NPs is primarily distributed between 10 and 20 nm. Since this size range is below the critical threshold for superparamagnetism in Fe3O4 (typically 25 nm), the nanoparticles are expected to exhibit superparamagnetic behavior [37,38]. Considering the particle size distribution of the Fe3O4 nanoparticles during sample preparation, a small fraction of the nanoparticles may form small clusters, whereas the majority of the nanoparticles satisfy the size criterion for superparamagnetic behavior. The SEM images reveal that the rGO maintains a single-layer, sheet-like structure. Through electrostatic adsorption, the Fe3O4 NPs clusters are effectively decorated onto the surface of the rGO nanosheets. Furthermore, as shown in Figure 3c, when an external magnetic field is applied, the Fe3O4-decorated rGO sheets exhibit a clear directional alignment along the magnetic field lines. This can be attributed to the fact that, under the influence of the external magnetic field, the nonzero average magnetic moments generated by the superparamagnetic Fe3O4 nanoparticles tend to align along the direction of the applied field, thereby driving the orientation of the Fe3O4/rGO composite sheets within the epoxy matrix. 3.2. Magnetic Characterization As shown in Figure 4a, the pure Fe3O4 nanoparticles (without rGO) exhibit remanence (Mr) and coercivity (Hc) values near zero, with no discernible hysteresis effect observed within the measurement range. The saturation magnetization (Ms) is relatively high, approximately 76 emu/g. As shown in the enlarged view of the low-magnetic-field region in Figure 4b, the pure Fe3O4 sample exhibits very small coercivity and remanent magnetization, with values of only 79 Oe and 6.5 emu/g, respectively. Taking into account instrumental uncertainty, particle size distribution, and possible aggregation effects, these results indicate that the sample exhibits typical superparamagnetic behavior at room temperature. With the increasing content of rGO in the composites, the Ms value gradually decreases to 68 emu/g. Nevertheless, the composites still maintain distinct superparamagnetic behavior [39]. The reduction in Ms is attributed to the introduction of the non-magnetic rGO phase, which reduces the overall magnetic mass fraction in the composites. 3.3. Electromagnetic Parameters of Composites The complex permittivity and permeability of the prepared Fe3O4/rGO composites were measured via the waveguide method in the frequency range of 8–12 GHz. Samples subjected to an external magnetic field are distinguished by the suffix “-H” in their labels. Figure 5a–f present the electromagnetic parameters of the Fe3O4/rGO composites. As shown in Figure 5a,b, the increasing weight ratio of rGO leads to a simultaneous enhancement in the real part of the complex permittivity, which rises from approximately 8 (SAMP-1) to over 20 (SAMP-3). Meanwhile, a corresponding increase in the imaginary part is also observed. Consequently, the dielectric loss tangent (tanδε=ε′′/ε′) is significantly improved (Figure 5c). Furthermore, the application of a magnetic field further enhances the dielectric loss capacity. This is attributed to the directional alignment of the rGO-based composites parallel to the incident electromagnetic waves, which creates a longer interaction path and results in stronger absorption [40]. These differences are more clearly illustrated by the Cole-Cole plots (Figure S3). The semicircles representing Debye relaxation become more prominent and increase in number with higher rGO content and the application of a magnetic field. This indicates that the abundant hetero-interfaces within the material trigger intensified interfacial polarization, thereby introducing additional relaxation processes [17,41]. Figure 5d–f illustrate the magnetic response characteristics of the Fe3O4/rGO composites. It is observed that the real part of the complex permeability decreases as the rGO content increases. This decline is primarily ascribed to the increased volume fraction of the non-magnetic phase (rGO), which leads to a “dilution effect” that weakens the overall magnetic energy storage capacity of the material. In contrast, the imaginary part and the magnetic loss tangent (tanδμ=μ″/μ′) exhibit an upward trend across most of the frequency range. This phenomenon can be explained by the fact that the introduction of more rGO nanosheets promotes a more uniform and sparse dispersion of Fe3O4, effectively preventing their agglomeration. The resulting increase in hetero-interfaces and the specific distribution of nanoparticles facilitate magnetic dissipation processes, such as natural resonance and superparamagnetic relaxation, thereby enhancing the magnetic loss capability [40]. Generally, the magnetic loss in magnetic materials primarily originates from hysteresis loss, domain wall resonance, eddy current loss, and natural resonance [4,42]. Among these, hysteresis loss and domain wall resonance typically occur under strong magnetic fields and at low frequencies; they are generally considered negligible in the microwave frequency range under the weak field conditions of a VNA measurement. Furthermore, domain wall resonance is exclusively associated with multi-domain materials. Given that the Fe3O4 nanoparticles in this study have a particle size of approximately 10–20 nm—below the critical threshold for multi-domain structures—they can be regarded as single-domain particles [37]. Consequently, neither hysteresis nor domain wall resonance contributes significantly to the observed loss. Eddy current loss refers to the energy dissipation caused by induced currents within a conductive material under an alternating magnetic field. It is proportional to the square of the frequency and represents a major component of magnetic loss at high frequencies. To determine whether the magnetic loss is solely dominated by the eddy current effect, the eddy current coefficient (C0) can be evaluated using the following relation [43].(1)C0=μ″μ′2f=23πμ0D2σ where D represents the diameter of the magnetic particles, while μ′ and μ″ denote the real and imaginary parts of the complex permeability of the material, respectively, μ0 is the permeability of free space, and σ is the material’s electrical conductivity. If the magnetic loss were solely attributed to eddy current loss, the C0 value should remain constant across the investigated frequency range. By substituting the experimental permeability parameters into the aforementioned equation, the C0 values for the 8–12 GHz range were calculated. As shown in Figure S4, the C0 values of all samples decrease markedly with increasing frequency. For example, the C0 value of SAMP-3 decreases from 0.025 at 8 GHz to 0.005 at 12 GHz, corresponding to a reduction of approximately 80%. A similar trend is also observed for the other samples. This trend clearly indicates that eddy current loss is not the dominant mechanism governing the magnetic dissipation. Considering that natural ferromagnetic resonance in magnetic nanomaterials typically occurs in the lower frequency range, it cannot fully account for the broadband response. According to the Kittel equation, the natural resonance relaxation expression for spherical magnetic particles is [44]:(2)fr=γHk2π where γ represents the gyromagnetic ratio, according to the cubic symmetry system, the equivalent magnetic crystal anisotropy field is Hk=4K13μ0Ms where the magnetic crystal anisotropy constant is K1=3.98×102 J/m3, and the saturation magnetization is Ms=3.63×105 A/m. The natural resonance frequency calculated from these parameters is 0.57 GHz. Furthermore, the broad peak distribution observed in the magnetic loss tangent is closely related to the wide particle size distribution of the superparamagnetic Fe3O4. Consequently, it can be inferred that the broadband magnetic response at high frequencies primarily originates from superparamagnetic relaxation [44].(3)fs=f0exp−KVkBT The relaxation frequency can be described by the Néel–Brown relaxation theory. In the related expression, f0 represents the attempt frequency, which denotes the number of times per second that the magnetic moment attempts to overcome the energy barrier in the absence of thermal energy. Since f0 is difficult to measure directly, a typical value ranging from 109–1011 Hz is generally adopted for ferrites [37]. K is the magnetocrystalline anisotropy constant, V is the size of the single-domain particle, kB is the Boltzmann constant, and T is the temperature. It is evident that the superparamagnetic relaxation frequency is strongly dependent on both particle size and temperature; specifically, it is inversely correlated with the particle volume (V) and positively correlated with the temperature (T). According to the Néel–Brown theory, the magnetic loss mechanism can be elucidated as follows: the emergence of magnetic loss peaks is primarily driven by the interaction between the Gilbert damping torque, generated during the reversal of magnetic moments under thermal fluctuations, and the externally applied alternating magnetic field [15]. 3.4. Improved Absorption Properties of Composites In the field of stealth technology, the minimum reflection loss (RLmin), effective absorption bandwidth (EAB, RL<−10 dB), and matching thickness are the most critical parameters for evaluating performance [45].(4)RL(dB)=20lg Zin−Z0Zin+Z0(5)Zin=Z0μrεrtanh j2πfdcμrεr Based on transmission line theory, Figure 6 displays the calculated RL contour maps for composites with different rGO contents. By increasing the weight fraction of rGO, the microwave absorption properties of the composites were significantly enhanced. The RLmin improved from −8.9 dB to −29.6 dB, while the EAB was simultaneously extended to cover the entire X-band (8–12 GHz). Furthermore, the application of an external magnetic field led to a distinct improvement in absorption performance across all doping ratios. Notably, when the rGO content reached 10 wt%, the material achieved full-band effective absorption (8–12 GHz) within a thickness range of 1–3 mm. Compared with the SAMP-3 sample prepared without an external magnetic field, the magnetically treated SAMP-3H sample exhibits superior microwave absorption performance. While maintaining effective absorption across the entire X-band, its minimum reflection loss is further enhanced from −29 dB to −40.3 dB. This result indicates that the magnetic-field-induced orientation significantly improves the electromagnetic wave attenuation capability of the composite. The superior electromagnetic wave attenuation capability of the material can be further elucidated by analyzing the impedance matching (Zin/Z0) and the attenuation constant (α) [46]. The impedance matching degree is characterized by the ratio of the material’s input impedance(Zin) to the impedance of free space(Zo), expressed as Zin/Z0. Generally, a Zin/Z0 value closer to 1 signifies that the material’s impedance is better matched to that of air, allowing incident electromagnetic waves to penetrate the interface more effectively rather than being reflected [47]. This facilitates stronger interaction between the waves and the material, leading to enhanced absorption and dissipation. As shown in Figure 7, Zin/Z0−1 is used to represent the degree of impedance matching. It is defined that Zin/Z0−1<0.2 indicates perfect impedance matching. By optimizing the rGO doping ratio, the dielectric loss and magnetic loss are effectively balanced, resulting in a significant enhancement of the impedance matching properties. Specifically, as shown in Figure 7c,f, when the rGO content reaches 10 wt%, the material achieves perfect matching at specific thicknesses and frequency bands. This phenomenon arises because rGO sheets oriented parallel to the direction of electromagnetic-wave propagation facilitate easier wave entry into the material compared to a disordered distribution. As shown in Figure S5, the α values of the composites increase with increasing rGO content, indicating enhanced electromagnetic wave attenuation capability within the materials. For example, the average α value increases from approximately 50 for SAMP-1 to approximately 90 for SAMP-3. In addition, within the frequency range of 8–12 GHz, SAMP-3 exhibits an average α value of approximately 90, whereas that of SAMP-3H increases to approximately 110, which is significantly higher than that of SAMP-3 prepared without an external magnetic field. These quantitative results further demonstrate that both the increased rGO content and the magnetic-field-induced orientation contribute to improving the electromagnetic attenuation capability of the composites. The increase in the attenuation constant (α) induced by the external magnetic field can be attributed to the fact that the parallel alignment of rGO sheets extends the interaction pathways between the material and incident electromagnetic waves, ultimately leading to enhanced absorption and increased energy dissipation. Compared with the microwave absorption performance of recently reported representative magnetic carbon-based absorbers listed in Table 2, the magnetic-field-induced enhanced Fe3O4/rGO composite proposed in this study achieves synergistic regulation of both composition and structure, exhibiting comprehensive advantages in microwave absorption, including a broad absorption bandwidth, a thin matching thickness, and strong reflection loss. Specifically, the minimum reflection loss reaches −40.3 dB at 8.79 GHz, and the effective absorption bandwidth (≤–10 dB) covers the entire 8–12 GHz range at a relatively thin matching thickness, outperforming most comparable materials. Finally, the microwave absorption mechanism is comprehensively elucidated in Figure 8. By fabricating the composite through the electrostatic adsorption of rGO and superparamagnetic Fe3O4 nanoparticles, the material integrates magnetic loss dominated by superparamagnetic relaxation with interfacial polarization arising from the abundant heterogeneous interfaces. Complemented by magnetic-field-induced oriented structures that extend the attenuation paths of electromagnetic waves, the composite achieves maximized electromagnetic wave absorption performance. 4. Conclusions In summary, a series of Fe3O4/rGO composites were synthesized, and the influences of rGO doping ratios and external magnetic fields on their electromagnetic response were thoroughly investigated. Through the electrostatic adsorption method, Fe3O4 nanoparticles were successfully anchored onto single-layer rGO sheets, while the oriented distribution of rGO within the material was achieved via an external magnetic field. Both experimental and calculated results demonstrate that the electromagnetic properties of the composites are highly enhanced by modulating the material ratios and magnetic field intensity. Notably, under an external magnetic field, the composite with a 10 wt% rGO doping ratio achieved effective absorption across the entire 8–12 GHz frequency range within a thickness of 1–3 mm, with a minimum reflection loss (RLmin) of −40.3 dB. This work provides a novel approach for the micro-nano-scale modulation of composites and offers promising new insights for the engineering of advanced microwave absorbing materials.